Martensitic stainless steel with high strength and toughness and preparation method thereof

Through process adjustments such as smelting, hot rolling, annealing, quenching-tempering, high-strength and toughness, high yield strength, tensile strength and resistance are achieved. Abrasiveness, suitable for tool use under severe working conditions.

CN118996236APending Publication Date: 2024-11-22TAIYUAN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192982.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing tools are difficult to balance between strength and toughness, especially in extreme working environments, and durability and reliability are difficult to ensure.

Method used

Through smelting, hot rolling, spherical annealing, cold rolling and quenching-tempering treatment, the composition and process flow of martensite stainless steel are adjusted to prepare high-strength and tough martensite stainless steel. The specific steps include smelting cast billets, hot rolling, annealing, and , cold rolling and quenching-tempering, control the content of elements such as C, Mo, V, and other V, and refine the grains through multi-pass hot rolling and cold rolling.

Benefits of technology

The prepared high-strength martensitic stainless steel has yield strength ≥1340MPa, tensile strength ≥1710MPa, elongation ≥8.0% and impact toughness ≥31J/cm2, hardness ≥51HRC, and is suitable for harsh working conditions such as high-speed cutting and dry cutting. , extend service life and improve work efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention belongs to the technical field of martensitic stainless steel, and particularly relates to high-strength and high-toughness martensitic stainless steel and a preparation method thereof.Component adjustment and production process improvement are conducted on the basis of traditional martensitic stainless steel, the high-strength and high-toughness martensitic stainless steel is prepared, the yield strength of the high-strength and high-toughness martensitic stainless steel is larger than or equal to 1340 MPa, the tensile strength is larger than or equal to 1710 MPa, and the ductility is larger than or equal to 8.0%; the impact toughness is not less than 31J / cm < 2 >. In addition, a tool prepared from the high-strength and high-toughness martensitic stainless steel has excellent wear resistance (the hardness is greater than or equal to 51 HRC), is particularly suitable for being used in high-speed cutting, dry cutting and other harsh working conditions, and can prolong the service life and improve the working efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of martensitic stainless steel, in particular to high-strength and toughness martensitic stainless steel and a preparation method thereof. Background Art

[0002] The cutting tools on the market today often have difficulty striking a balance between strength and toughness, especially in extreme working environments, where the durability and reliability of cutting tools have become key issues that need to be addressed. Although researchers in Germany, Japan and other countries have developed a series of high-performance stainless steel materials for cutting tools through complex alloy design and sophisticated heat treatment processes, it is still difficult for cutting tools to strike an ideal balance between strength and toughness. Therefore, it is particularly important to develop a martensitic stainless steel cutting tool material that has both high strength and high toughness. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a high-strength and toughness martensitic stainless steel and a preparation method thereof.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A method for preparing high-strength and high-toughness martensitic stainless steel comprises the following steps:

[0006] S1, smelting and casting to obtain a casting billet;

[0007] S2, hot rolling the ingot to obtain a hot-rolled plate;

[0008] S3, performing spheroidizing annealing on the hot rolled plate;

[0009] S4, cold rolling the annealed hot-rolled sheet to obtain a cold-rolled sheet;

[0010] S5. The cold-rolled sheet is subjected to quenching-tempering treatment, wherein the quenching austenitizing temperature is 950-1030° C., and the holding time is 5-8 min; the quenching method is water cooling; the tempering temperature is 240-260° C., and the holding time is 30-40 min; and the high-strength and toughness martensitic stainless steel is obtained after air cooling, wherein the C element content of the high-strength and toughness martensitic stainless steel is 0.32-0.35wt%, the Mo element content is 0.1-0.2wt%, and the V element content is 0.1-0.15wt%.

[0011] As a preferred embodiment of the method for preparing high-strength and toughness martensitic stainless steel described in the present invention, wherein: in the step S2, the ingot is heated to 1150-1200°C, kept warm for 100-120 minutes, and then subjected to multiple rapid and continuous hot rolling to obtain a 3.8-4.2 mm plate, the final rolling temperature is 855-865°C, the total reduction is 94-95%, and the plate is air-cooled to room temperature after hot rolling.

[0012] As a preferred embodiment of the method for preparing high-strength and toughness martensitic stainless steel described in the present invention, in step S3, the annealing process is: first, keep warm at 875-895°C for 55-75 minutes, then cool to 575-595°C with the furnace, and then air-cool to room temperature.

[0013] As a preferred embodiment of the method for preparing high-strength and toughness martensitic stainless steel described in the present invention, in step S4, multiple passes of continuous cold rolling are performed to obtain 1.4 mm to 1.6 mm plates with a total reduction of 60 to 65%.

[0014] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0015] A high-strength and toughness martensitic stainless steel is prepared by adopting the above-mentioned high-strength and toughness martensitic stainless steel preparation method.

[0016] As a preferred embodiment of the high-strength and toughness martensitic stainless steel described in the present invention, the composition of the high-strength and toughness martensitic stainless steel includes, by mass percentage, C: 0.32-0.35%, Cr: 12.5-13.5%, Mn: 0.4-0.6%, Si: 0.4-0.6%, Mo: 0.1-0.2%, V: 0.1-0.15%, Ni: 0.2-0.3%, P<0.01%, S<0.01%, and the balance is Fe and unavoidable impurity elements.

[0017] As a preferred embodiment of the high-strength and toughness martensitic stainless steel described in the present invention, the carbide size of the high-strength and toughness martensitic stainless steel is 145-505 nm, and the grain size of the high-strength and toughness martensitic stainless steel is 5.5-8.5 μm.

[0018] As a preferred embodiment of the high-strength and toughness martensitic stainless steel of the present invention, the yield strength of the high-strength and toughness martensitic stainless steel is ≥1340MPa, the tensile strength is ≥1710MPa, the elongation is ≥8.0%, and the impact toughness is ≥31J / cm 2 , hardness ≥51HRC.

[0019] The beneficial effects of the present invention are as follows:

[0020] The present invention provides a high-strength and tough martensitic stainless steel and a preparation method thereof. The composition of the conventional martensitic stainless steel is adjusted and the production process is improved to prepare the high-strength and tough martensitic stainless steel. The high-strength and tough martensitic stainless steel has a yield strength of ≥1340MPa, a tensile strength of ≥1710MPa, an elongation of ≥8.0%, and an impact toughness of ≥31J / cm 2 In addition, the cutting tool made of the high-strength and tough martensitic stainless steel of the present invention also exhibits excellent wear resistance (hardness ≥ 51HRC), and is particularly suitable for use in cutting tools under harsh working conditions such as high-speed cutting and dry cutting, which can extend the service life and improve work efficiency. DETAILED DESCRIPTION

[0021] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] According to one aspect of the present invention, the present invention provides the following technical solution:

[0023] A method for preparing high-strength and high-toughness martensitic stainless steel comprises the following steps:

[0024] S1, smelting and casting to obtain a casting billet;

[0025] S2, hot rolling the ingot to obtain a hot-rolled plate;

[0026] S3, performing spheroidizing annealing on the hot rolled plate;

[0027] S4, cold rolling the annealed hot-rolled sheet to obtain a cold-rolled sheet;

[0028] S5. The cold-rolled sheet is subjected to quenching-tempering treatment, wherein the quenching austenitizing temperature is 950-1030° C., and the holding time is 5-8 min; the quenching method is water cooling; the tempering temperature is 240-260° C., and the holding time is 30-40 min; and the high-strength and toughness martensitic stainless steel is obtained after air cooling, wherein the C element content of the high-strength and toughness martensitic stainless steel is 0.32-0.35wt%, the Mo element content is 0.1-0.2wt%, and the V element content is 0.1-0.15wt%.

[0029] Preferably, in step S2, the ingot is heated to 1150-1200°C, kept warm for 100-120 minutes, and then subjected to multiple passes of rapid and continuous hot rolling to obtain a 3.8-4.2 mm plate, with a final rolling temperature of 855-865°C, a total reduction of 94-95%, and air cooling to room temperature after hot rolling. The plasticity of the plate is improved by hot rolling, the thickness and shape of the material are adjusted, and the grains are refined by hot working, laying the foundation for subsequent cold rolling and final performance. Specifically, the heating temperature may be, for example, any one of 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, or a range between any two thereof; the final rolling temperature may be, for example, any one of 855°C, 860°C, 865°C, or a range between any two thereof.

[0030] Preferably, in step S3, the annealing process is: first, keep the temperature at 875-895°C for 55-75 minutes, then cool to 575-595°C with the furnace, and then air cool to room temperature. The annealing process is intended to eliminate work hardening, restore the plasticity of the material, prepare for cold rolling, and homogenize the internal structure. Specifically, the holding temperature can be, for example, any one of 875°C, 880°C, 885°C, 890°C, 895°C, or a range between any two of them.

[0031] Preferably, in step S4, the annealed sheet is pickled and shot peened to remove defects such as scale and rust spots on the surface of the sheet, making the surface smooth and clean, and then multiple continuous cold rolling is performed to obtain a 1.4mm~1.6mm sheet with a total reduction of 60~65%. The cold rolling further refines the grains, improves the strength and hardness of the material, and controls the size and surface quality of the sheet. Specifically, the total cold rolling reduction can be, for example, any one of 60%, 61%, 62%, 63%, 64%, 65%, or a range between any two.

[0032] According to another aspect of the present invention, the present invention provides the following technical solution:

[0033] A high-strength and toughness martensitic stainless steel is prepared by adopting the above-mentioned high-strength and toughness martensitic stainless steel preparation method.

[0034] Preferably, the composition of the high-strength and toughness martensitic stainless steel includes, by mass percentage, C: 0.32~0.35%, Cr: 12.5~13.5%, Mn: 0.4~0.6%, Si: 0.4~0.6%, Mo: 0.1~0.2%, V: 0.1~0.15%, Ni: 0.2~0.3%, P<0.01%, S<0.01%, and the balance is Fe and unavoidable impurity elements.

[0035] Carbon (C) is crucial to improving the hardness and strength of steel materials. It exhibits strong solid solution strengthening and precipitation strengthening effects. When it is less than 0.32wt%, the hardness and strength of the material are relatively mediocre; on the contrary, when it is greater than 0.35wt%, it is easy to cause the enrichment of carbon chromium and form chromium-poor areas, thereby weakening the corrosion resistance of the material.

[0036] Chromium (Cr) is a key element for stainless steel to resist corrosion. A thin and dense chromium oxide (Cr2O3) passivation film will be formed on the surface of the material. The formation of this passivation film is particularly effective when the content is not less than 12.5wt%. At the same time, too much chromium also helps to form a stable ferrite phase, which limits hot workability. Therefore, its content should not exceed 13.5 wt%.

[0037] An appropriate amount of manganese (Mn, 0.4~0.6 wt%) can increase the strength and hardness of steel, but too high a content (>0.6wt%) will increase the brittleness of the material and reduce its toughness. At the same time, as an effective desulfurizer, manganese will be less effective if the content is too low (<0.4wt%).

[0038] Silicon (Si) is a highly efficient deoxidizer. If its content is too high (>0.6wt%), the austenite phase area will be reduced, ferrite will be more easily formed, and the mechanical properties will be weakened. If the content is too low (<0.4wt%), it will be detrimental to the removal of oxide impurities and the purity of stainless steel.

[0039] The addition of molybdenum (Mo) can enhance the corrosion resistance and solid solution strengthening properties of the material, while optimizing the hardenability and processability of the steel, promoting grain refinement and enhancing toughness. If the content is less than 0.1wt%, the strengthening effect is negligible; in view of the precious properties of molybdenum, considering the comprehensive cost-effectiveness, the upper limit of its content is preferably set at 0.2wt%.

[0040] Vanadium (V) is a strong carbide-forming element. Usually, a content of more than 0.1wt% can promote grain refinement and improve the strength and toughness of the material. Excessive vanadium content (>0.15wt%) will promote the precipitation of hard and brittle carbides, thereby affecting the toughness of the material.

[0041] Nickel (Ni) performs well in expanding the austenite phase and enhancing the stability of austenite, effectively reducing the ductile-brittle transition temperature of steel and enhancing toughness. However, excessive nickel content (>0.3wt%) will lead to an increase in retained austenite and a decrease in strength.

[0042] Phosphorus (P) and sulfur (S) are two elements that tend to segregate at grain boundaries, which is detrimental to hot working properties. Therefore, their content in steel should be minimized.

[0043] Preferably, the carbide size of the high-strength and toughness martensitic stainless steel is 145-505 nm, and the grain size of the high-strength and toughness martensitic stainless steel is 5.5-8.5 μm.

[0044] Preferably, the high-strength and tough martensitic stainless steel has a yield strength of ≥1340 MPa, a tensile strength of ≥1710 MPa, an elongation of ≥8.0%, and an impact toughness of ≥31 J / cm 2 , hardness ≥51HRC.

[0045] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0046] Example 1

[0047] A method for preparing high-strength and high-toughness martensitic stainless steel comprises the following steps:

[0048] S1, smelting and casting to obtain a casting billet;

[0049] S2, heating the ingot to 1200°C, keeping the temperature for 120 minutes, and then performing multiple rapid and continuous hot rolling to obtain a 4.0 mm plate, with a final rolling temperature of 860°C and a total reduction of 94.6%, and air cooling to room temperature after hot rolling;

[0050] S3, spheroidizing annealing is performed on the hot-rolled plate; the annealing process is: first, keep the temperature at 890°C for 60 minutes, then cool to 590°C with the furnace, and then air cool to room temperature;

[0051] S4, pickling and shot peening the annealed plate to remove the oxide scale, rust spots and other defects on the surface of the plate to make the surface smooth and clean, and then perform multiple continuous cold rolling to obtain 1.5mm plate with a total reduction of 62.5%;

[0052] S5. The cold-rolled sheet is subjected to quenching-tempering treatment, wherein the quenching austenitizing temperature is 950° C. and the holding time is 5 min; the quenching method is water cooling; the tempering temperature is 250° C. and the holding time is 30 min; and the high-strength and toughness martensitic stainless steel is obtained after air cooling.

[0053] The composition of the high-strength and tough martensitic stainless steel prepared in this embodiment is shown in Table 1:

[0054] Table 1 Composition of high-strength and tough martensitic stainless steel of Example 1 (mass percentage, wt%)

[0055]

[0056] Example 2

[0057] The difference from Example 1 is that in step S5, the austenitizing temperature is 990°C.

[0058] Example 3

[0059] The difference from Example 1 is that in step S5, the austenitizing temperature is 1030°C.

[0060] Comparative Example 1

[0061] The difference from Example 1 is that a commercial 30Cr13 cold-rolled sheet is used.

[0062] Comparative Example 2

[0063] The difference from Example 2 is that a commercial 30Cr13 cold-rolled sheet is used.

[0064] Comparative Example 3

[0065] The difference from Example 3 is that a commercial 30Cr13 cold-rolled sheet is used.

[0066] Comparative Example 4

[0067] The difference from Example 1 is that the austenitizing temperature in step S5 is 1050°C.

[0068] Comparative Example 5

[0069] The difference from Example 1 is that the tempering temperature in step S5 is 200°C.

[0070] Comparative Example 6

[0071] The difference from Example 1 is that in step S3, the temperature is kept at 850° C. for 60 minutes.

[0072] Comparative Example 7

[0073] The difference from Example 1 is that the Mo element content is 1.0 wt %.

[0074] Comparative Example 8

[0075] The difference from Example 1 is that the V element content is 0.4 wt %.

[0076] Comparative Example 9

[0077] The difference from Example 1 is that Mo and V are not contained.

[0078] The properties of the martensitic stainless steel obtained in the examples of the present invention and the comparative examples were tested, and the results are shown in Table 2:

[0079] Table 2 Properties of martensitic stainless steel obtained in Examples and Comparative Examples

[0080]

[0081] As can be seen from Table 2, the present invention adjusts the composition and improves the production process on the basis of traditional martensitic stainless steel to prepare high-strength and tough martensitic stainless steel, wherein the yield strength of the high-strength and tough martensitic stainless steel is ≥1340MPa, the tensile strength is ≥1710MPa, the elongation is ≥8.0%, and the impact toughness is ≥31J / cm 2 In addition, the cutting tool made of the high-strength and tough martensitic stainless steel of the present invention also exhibits excellent wear resistance (hardness ≥ 51HRC), and is particularly suitable for use in cutting tools under harsh working conditions such as high-speed cutting and dry cutting, which can extend the service life and improve work efficiency.

[0082] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing high-strength and high-toughness martensitic stainless steel, characterized in that: The steps include: S1, smelting and casting to obtain a casting billet; S2, hot rolling the ingot to obtain a hot-rolled plate; S3, performing spheroidizing annealing on the hot rolled plate; S4, cold rolling the annealed hot-rolled sheet to obtain a cold-rolled sheet; S5. The cold-rolled sheet is subjected to quenching-tempering treatment, wherein the quenching austenitizing temperature is 950-1030° C., and the holding time is 5-8 min; the tempering temperature is 240-260° C., and the holding time is 30-40 min; and the high-strength and toughness martensitic stainless steel is obtained after air cooling, wherein the C element content of the high-strength and toughness martensitic stainless steel is 0.32-0.35wt%, the Mo element content is 0.1-0.2wt%, and the V element content is 0.1-0.15wt%.

2. The method for preparing high-strength and tough martensitic stainless steel according to claim 1, characterized in that: In step S2, the ingot is heated to 1150-1200°C, kept warm for 100-120 minutes, and then subjected to multiple rapid and continuous hot rolling to obtain a 3.8-4.2 mm plate. The final rolling temperature is 855-865°C, the total reduction is 94-95%, and the plate is air-cooled to room temperature after hot rolling.

3. The method for preparing high-strength and tough martensitic stainless steel according to claim 1, characterized in that: In step S3, the annealing process is: first, keep the temperature at 875-895° C. for 55-75 min, then cool to 575-595° C. with the furnace, and then air cool to room temperature.

4. The method for preparing high-strength and tough martensitic stainless steel according to claim 1, characterized in that: In the step S4, multiple continuous cold rolling passes are performed to obtain 1.4 mm to 1.6 mm plates with a total reduction of 60 to 65%.

5. The method for preparing high-strength and tough martensitic stainless steel according to claim 1, characterized in that: In the step S5, the quenching method is water cooling.

6. A high-strength and tough martensitic stainless steel, characterized in that: The high-strength and toughness martensitic stainless steel is prepared by the preparation method of any one of claims 1 to 5.

7. The high-strength and tough martensitic stainless steel according to claim 6, characterized in that: The composition of the high-strength and toughness martensitic stainless steel includes, in percentage by mass, C: 0.32-0.35%, Cr: 12.5-13.5%, Mn: 0.4-0.6%, Si: 0.4-0.6%, Mo: 0.1-0.2%, V: 0.1-0.15%, Ni: 0.2-0.3%, P<0.01%, S<0.01%, and the remainder is Fe and unavoidable impurity elements.

8. The high-strength and tough martensitic stainless steel according to claim 6, characterized in that: The carbide size of the high-strength and toughness martensitic stainless steel is 145-505 nm, and the grain size of the high-strength and toughness martensitic stainless steel is 5.5-8.5 μm.

9. The high-strength and tough martensitic stainless steel according to claim 6, characterized in that: The high-strength and tough martensitic stainless steel has a yield strength of ≥1340MPa, a tensile strength of ≥1710MPa, an elongation of ≥8.0%, and an impact toughness of ≥31J / cm 2 , hardness ≥51HRC.