Nodular cast iron casting process

Through scrap steel and other material ingredients and spheroidization incubation technology, combined with V-method casting technology, the problem that existing ductile iron cannot meet the requirements of high strength and high plasticity is solved, and the production of ductile iron with high strength and high elongation is achieved, reducing costs and simplifying The process flow supports the thin-wall and lightweight development of automotive parts.

CN118996247AInactive Publication Date: 2024-11-22JILIN WEICHUANG ELECTROMECHANICAL ENG CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310549627.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing ductile iron standards cannot meet the needs of high-strength, high-plastic cast ductile iron parts. The traditional production methods are costly and depend on heat treatment, making it difficult to achieve the development of thin-walled and lightweight automotive parts.

Method used

Using scrap steel, furnace recharge, carbon enhancer, silicon carbide and other materials, and through spheroidization incubation and V-measure casting processes, Si, Cu-Sn-Sb alloy elements and negative pressure conditions are controlled to achieve high-strength, high-plastic ductile iron Production avoids heat treatment steps and simplifies the process flow.

Benefits of technology

It significantly improves the comprehensive mechanical properties of ductile iron, meets the requirements of high strength and high elongation, reduces production costs, simplifies the process flow, and supports the thin-wall and lightweight development of automotive parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996247A_ABST
    Figure CN118996247A_ABST
Patent Text Reader

Abstract

The invention discloses a nodular cast iron casting process which comprises the following steps: S1, burdening: burdening; s2, feeding and smelting, and paving a layer of steel cuttings at the bottom of the furnace; s3, measuring the temperature, sampling and testing, heating to a certain temperature after the furnace burden is completely melted down, and then measuring the temperature, slagging off and sampling; s4, spheroidizing and inoculation are conducted, wherein 1.3% of a spheroidizing agent is added into a spheroidizing ladle bottom groove to be tamped; s5, pouring: pouring the molten iron into a sand casting mold manufactured by a V-method process after the temperature is measured to be qualified; and S6, pressure maintaining and mold dismantling are conducted, standing is conducted for a period of time after pouring is completed, and the negative pressure value is rapidly adjusted to be in the minimum state. The components and the manufacturing process are optimized, a cast material is obtained, the comprehensive mechanical property of the material is greatly improved, the requirements of a casting product for high strength and high elongation of nodular cast iron are met, the blank of a high-strength and high-plasticity production technology is filled up, and powerful support is provided for thin-wall and light-weight development of automobile part castings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of casting technology, in particular to a ductile iron casting technology. Background Art

[0002] With the development of industry, people have higher and higher requirements for the comprehensive performance of ductile iron. Traditional automobile chassis parts such as bridge housing, differential housing, wheel hub, balance suspension, crossbeam, etc. are all cast with ductile iron. The main failure mode of these parts during use is fatigue damage, and fatigue life is mainly related to strength and plasticity. Moreover, with the development of energy conservation and emission reduction, and automobile weight reduction, these chassis parts castings are developing towards thin-walled and lightweight. Therefore, the ductile iron used has higher strength and plasticity, ensuring a longer service life and higher safety and reliability during heavy-load operation.

[0003] At present, the general ductile iron national standard GB / T1348-2009 "Ductile Iron Parts" stipulates that there are 14 grades of ductile iron parts from QT350-22 to QT900-2. These grades of products generally have the common characteristics of low strength and high elongation or high strength and low elongation, which can no longer meet our needs for high-strength and high-plasticity cast ductile iron parts. Isothermal quenching ductile iron, also known as ADI, has higher strength and plasticity, and its performance is basically comparable to that of low-alloy steel, but it needs to be achieved through heat treatment, which is very expensive. The SiboDur ductile iron parts developed by GF are high-strength and high-elongation ductile iron in the cast state. The SiboDur450-17, SiboDur550-12, SiboDur700-10 and SiboDur800-5 series grades have been formed. What we can collect are some industrial reports, and there are few specific process technology data and literature. It mainly uses Si and B as alloying elements, with a specific tensile strength of 800MPa and an elongation that is difficult to reach 10%. Summary of the invention

[0004] The object of the present invention is to provide a ductile iron casting process to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: a ductile iron casting process, comprising the following steps:

[0006] S1: batching, according to the mass percentage, 60-65% of scrap steel, 35-40% of recycled materials, 2-3% of recarburizer, and 1% of silicon carbide are batched;

[0007] S2: Charge and smelt. Spread a layer of steel scraps on the bottom of the furnace, add scrap steel and start electric smelting. When a certain depth of molten iron appears at the bottom of the furnace, add 40% of the required carburizer. Add the remaining carburizer gradually while melting. When 1 / 3 to 1 / 2 of all the furnace materials are melted, add silicon carbide. Finally, add the return materials according to the smelting situation.

[0008] S3: temperature measurement, sampling, and testing. After the charge is completely melted, the temperature is raised to a certain temperature, and then the temperature is measured, slag is removed, and sampling is performed. After the composition is adjusted to meet the requirements, the temperature is raised again. After slag removal, the power is turned off and the charge is left to stand for removal from the furnace.

[0009] S4: Spheroidizing and inoculating. 1.3% of spheroidizing agent is added to the bottom trough of the spheroidizing ladle and compacted. Then, 0.6% of the homemade Si-Ba-Ca-Sn-Sb alloy composite inoculant is added to completely cover the spheroidizing agent. Then, 3 kg of iron filings are added to completely cover the inoculant and compact it. After the spheroidizing reaction is completed, the slag is removed. Then, the molten iron is quickly poured into the prepared casting ladle. Before pouring the molten iron, 0.4% of 75 ferrosilicon alloy inoculant is placed in the casting ladle in advance. After removing the slag again, it is hoisted to the casting station.

[0010] S5: pouring. After the temperature measurement is qualified, the molten iron is poured into the sand casting mold made by the V-method process. During the pouring process, the flow is instantaneously inoculated. The amount added is about 0.1% of the amount of molten iron. The pouring is completed within a period of time after the spheroidization reaction.

[0011] S6: Maintaining pressure and boxing. After pouring, let it stand for a while, quickly adjust the negative pressure value to the minimum state, maintain the pressure for a while, turn off the negative pressure, continue to keep warm for a while and then box, you can get high-strength and high-plasticity ductile iron material.

[0012] Preferably, in step S1, the mass percentage is adjusted as follows:

[0013] C:3.6—3.85; Si:2.4—2.8; Mn:0.3—0.5; P:≤0.03; S:≤0.02; Cu:0.4—0.5; Sn:0.02—0.08; Sb:0.01—0.04; Mg:0.04—0.06; RE:0.015—0.04; the rest is Fe.

[0014] Preferably, in step S1, the raw materials used in production include 08 aluminum scrap steel briquettes, recycled iron, recarburizer, and silicon carbide.

[0015] Preferably, in step S4, the spheroidizing inoculation process adopts Mg6RE2 spheroidizing agent, homemade Si-Ba-Ca-Sn-Sb alloy composite inoculant, ladle injection method for primary inoculation, 75 ferrosilicon alloy inverted injection method for secondary inoculation, and high-efficiency flow inoculation treatment, and the required proportion of ferrite and pearlite matrix is ​​obtained by controlling Sn and Sb and adjusting Si, Mn, and Cu contents, and adopts V-method casting process. After pouring, the cooling rate of the casting and the unpacking time are controlled by adjusting the size of the negative pressure and the pressure extraction time to refine the grains.

[0016] Preferably, in step S2, the laying area of ​​the steel chips is 100 mm±10 mm, and when molten iron with a depth of 100 mm appears at the bottom of the furnace, the required carburizer is added.

[0017] Preferably, in step S3, the first temperature rise needs to be within the range of 1410-1430°C, the adjusted second temperature rise needs to be above 1550°C, and the particle size range of the spheroidizing agent is 8-25 mm.

[0018] Preferably, in step S4, the particle size range of the 75 ferrosilicon alloy inoculant is 3-8 mm.

[0019] Preferably, in step S5, the negative pressure value needs to be adjusted to between -0.06 MPa and -0.045 MPa before pouring.

[0020] Preferably, in step S6, the standing time after pouring is 6-8 minutes, the pressure holding time is 15 minutes, and the heat preservation time is 10 minutes.

[0021] Technical effects and advantages of the present invention:

[0022] (1) The present invention optimizes the composition and manufacturing process to obtain a cast material, greatly improving the comprehensive mechanical properties of the material, meeting the requirements of casting products for ductile iron with high strength and high elongation, filling the gap in high-strength and high-plasticity production technology, and providing strong support for the development of automotive parts castings towards thin-walled and lightweight. The present invention uses Si elements to control the amount of ferrite in the matrix to ensure the plasticity of the material, and uses Cu-Sn-Sb alloy elements to regulate the pearlite content of the matrix. By controlling the size and time of negative pressure, the cooling rate of the casting is controlled and the box is timely beaten to refine the microstructure grains, thereby realizing stable mass production under cast conditions;

[0023] (2) The present invention uses scrap steel carburization technology to produce ductile iron, which changes the traditional production method of using high-purity pig iron as the main material to produce ductile iron. In addition, no precious elements such as Mo and Ni are used, and only trace amounts of Sn and Sb are added. The purpose of adjusting and controlling the graphite morphology, matrix structure, and comprehensive performance is achieved through microalloying, which greatly saves costs and significantly improves the economic benefits of the enterprise.

[0024] (3) The present invention does not require energy-consuming and time-consuming heat treatment and can be used directly in the cast state, which can simplify the production process, reduce energy consumption, and is simple to operate and stably control product quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is one of the metallographic organization diagrams of the present invention.

[0026] Figure 2 This is the second metallographic organization diagram of the present invention.

[0027] Figure 3 This is the third metallographic organization diagram of the present invention.

[0028] Figure 4 This is the fourth metallographic organization diagram of the present invention.

[0029] Figure 5 This is the fifth metallographic organization diagram of the present invention.

[0030] Figure 6 This is the sixth metallographic organization diagram of the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] like Figure 1-2 The ductile iron casting process shown includes the following steps:

[0034] S1: batching, according to the mass percentage, 60-65% of scrap steel, 35-40% of recycled materials, 2-3% of recarburizer, and 1% of silicon carbide are batched;

[0035] S2: Charge and smelt. Spread a layer of steel scraps on the bottom of the furnace, add scrap steel and start electric smelting. When a certain depth of molten iron appears at the bottom of the furnace, add 40% of the required carburizer. Add the remaining carburizer gradually while melting. When 1 / 3 to 1 / 2 of all the furnace materials are melted, add silicon carbide. Finally, add the return materials according to the smelting situation.

[0036] S3: temperature measurement, sampling, and testing. After the charge is completely melted, the temperature is raised to a certain temperature, and then the temperature is measured, slag is removed, and sampling is performed. After the composition is adjusted to meet the requirements, the temperature is raised again. After slag removal, the power is turned off and the charge is left to stand for removal from the furnace.

[0037] S4: Spheroidizing and inoculating. 1.3% of spheroidizing agent is added to the bottom trough of the spheroidizing ladle and compacted. Then, 0.6% of the homemade Si-Ba-Ca-Sn-Sb alloy composite inoculant is added to completely cover the spheroidizing agent. Then, 3 kg of iron filings are added to completely cover the inoculant and compact it. After the spheroidizing reaction is completed, the slag is removed. Then, the molten iron is quickly poured into the prepared casting ladle. Before pouring the molten iron, 0.4% of 75 ferrosilicon alloy inoculant is placed in the casting ladle in advance. After removing the slag again, it is hoisted to the casting station.

[0038] S5: pouring. After the temperature measurement is qualified, the molten iron is poured into the sand casting mold made by the V-method process. During the pouring process, the flow is instantaneously inoculated. The amount added is about 0.1% of the amount of molten iron. The pouring is completed within a period of time after the spheroidization reaction.

[0039] S6: Maintaining pressure and boxing. After pouring, let it stand for a while, quickly adjust the negative pressure value to the minimum state, maintain the pressure for a while, turn off the negative pressure, continue to keep warm for a while and then box, you can get high-strength and high-plasticity ductile iron material.

[0040] In step S1, the mass percentage is adjusted as follows:

[0041] C:3.68, Si:2.79, Mn:0.35, Cu:0.41, P:0.05, S:0.009, RE:0.018, Mg:0.043, Sn:0.034, Sb:0.015, and the rest is Fe.

[0042] In step S1, the raw materials used in production include 08 aluminum scrap steel briquettes, recycled iron, carburizer, and silicon carbide.

[0043] In step S4, the spheroidizing inoculation process adopts Mg6RE2 spheroidizing agent, homemade Si-Ba-Ca-Sn-Sb alloy composite inoculant, ladle injection method for primary inoculation, 75 ferrosilicon alloy inverted injection method for secondary inoculation, and high-efficiency flow inoculation treatment. The required proportion of ferrite and pearlite matrix is ​​obtained by controlling Sn and Sb and adjusting Si, Mn, and Cu contents. The V casting process is adopted. After pouring, the cooling rate of the casting is controlled by adjusting the size of the negative pressure and the pressure extraction time, and the grain is refined by the unpacking time.

[0044] In step S2, the laying area of ​​the steel chips is 100 mm ± 10 mm, and when molten iron with a depth of 100 mm appears at the bottom of the furnace, the required carburizer is added.

[0045] In step S3, the first temperature rise needs to be within the range of 1410-1430°C, the adjusted second temperature rise needs to be above 1550°C, and the particle size range of the spheroidizing agent is 8-25 mm.

[0046] In step S4, the particle size of the 75 ferrosilicon alloy inoculant is in the range of 3-8 mm.

[0047] In step S5, the negative pressure value needs to be adjusted to between -0.06 MPa and -0.045 MPa before pouring.

[0048] In step S6, after pouring, the standing time is 6-8 minutes, the pressure holding time is 15 minutes, and the heat preservation time is 10 minutes.

[0049] The mechanical properties of the main test bar are: hardness 256HB, 247HB, tensile strength σb = 817MPa, 807MPa, yield strength σ0.2 = 457MPa, 442MPa, elongation δ = 11.2%, 11.8%. Its metallographic structure is as follows Figure 1-2 As shown: spheroidization level 2-3, ball diameter level 6-8, pearlite content 65%.

[0050] Example 2

[0051] like Figure 3-4 The ductile iron casting process shown includes the following steps:

[0052] S1: batching, according to the mass percentage, 60-65% of scrap steel, 35-40% of recycled materials, 2-3% of recarburizer, and 1% of silicon carbide are batched;

[0053] S2: Charge and smelt. Spread a layer of steel scraps on the bottom of the furnace, add scrap steel and start electric smelting. When a certain depth of molten iron appears at the bottom of the furnace, add 40% of the required carburizer. Add the remaining carburizer gradually while melting. When 1 / 3 to 1 / 2 of all the furnace materials are melted, add silicon carbide. Finally, add the return materials according to the smelting situation.

[0054] S3: temperature measurement, sampling, and testing. After the charge is completely melted, the temperature is raised to a certain temperature, and then the temperature is measured, slag is removed, and sampling is performed. After the composition is adjusted to meet the requirements, the temperature is raised again. After slag removal, the power is turned off and the charge is left to stand for removal from the furnace.

[0055] S4: Spheroidizing and inoculating. 1.3% of spheroidizing agent is added to the bottom trough of the spheroidizing ladle and compacted. Then, 0.6% of the homemade Si-Ba-Ca-Sn-Sb alloy composite inoculant is added to completely cover the spheroidizing agent. Then, 3 kg of iron filings are added to completely cover the inoculant and compact it. After the spheroidizing reaction is completed, the slag is removed. Then, the molten iron is quickly poured into the prepared casting ladle. Before pouring the molten iron, 0.4% of 75 ferrosilicon alloy inoculant is placed in the casting ladle in advance. After removing the slag again, it is hoisted to the casting station.

[0056] S5: pouring. After the temperature measurement is qualified, the molten iron is poured into the sand casting mold made by the V-method process. During the pouring process, the flow is instantaneously inoculated. The amount added is about 0.1% of the amount of molten iron. The pouring is completed within a period of time after the spheroidization reaction.

[0057] S6: Maintaining pressure and boxing. After pouring, let it stand for a while, quickly adjust the negative pressure value to the minimum state, maintain the pressure for a while, turn off the negative pressure, continue to keep warm for a while and then box, you can get high-strength and high-plasticity ductile iron material.

[0058] In step S1, the mass percentage is adjusted as follows:

[0059] C:3.65, Si:2.73, Mn:0.32, Cu:0.38, P:0.05, S:0.012, RE:0.015, Mg:0.045, Sn:0.030, Sb:0.01, and the rest is Fe.

[0060] In step S1, the raw materials used in production include 08 aluminum scrap steel briquettes, recycled iron, carburizer, and silicon carbide.

[0061] In step S4, the spheroidizing inoculation process adopts Mg6RE2 spheroidizing agent, homemade Si-Ba-Ca-Sn-Sb alloy composite inoculant, ladle injection method for primary inoculation, 75 ferrosilicon alloy inverted injection method for secondary inoculation, and high-efficiency flow inoculation treatment. The required proportion of ferrite and pearlite matrix is ​​obtained by controlling Sn and Sb and adjusting Si, Mn, and Cu contents. The V casting process is adopted. After pouring, the cooling rate of the casting is controlled by adjusting the size of the negative pressure and the pressure extraction time, and the grain is refined by the unpacking time.

[0062] In step S2, the laying area of ​​the steel chips is 100 mm ± 10 mm, and when molten iron with a depth of 100 mm appears at the bottom of the furnace, the required carburizer is added.

[0063] In step S3, the first temperature rise needs to be within the range of 1410-1430°C, the adjusted second temperature rise needs to be above 1550°C, and the particle size range of the spheroidizing agent is 8-25 mm.

[0064] In step S4, the particle size of the 75 ferrosilicon alloy inoculant is in the range of 3-8 mm.

[0065] In step S5, the negative pressure value needs to be adjusted to between -0.06 MPa and -0.045 MPa before pouring.

[0066] In step S6, after pouring, the standing time is 6-8 minutes, the pressure holding time is 15 minutes, and the heat preservation time is 10 minutes.

[0067] Hardness 262HB, 254HB, tensile strength σb = 831MPa, 822MPa, yield strength σ0.2 = 454MPa, 446MPa, elongation δ = 12.1%, 11.5%. Its metallographic structure is as follows Figure 3-4As shown: spheroidization level 2-3, ball diameter level 6-8, pearlite volume 70%.

[0068] Example 3

[0069] like Figure 5-6 The ductile iron casting process shown includes the following steps:

[0070] S1: batching, according to the mass percentage, 60-65% of scrap steel, 35-40% of recycled materials, 2-3% of recarburizer, and 1% of silicon carbide are batched;

[0071] S2: Charge and smelt. Spread a layer of steel scraps on the bottom of the furnace, add scrap steel and start electric smelting. When a certain depth of molten iron appears at the bottom of the furnace, add 40% of the required carburizer. Add the remaining carburizer gradually while melting. When 1 / 3 to 1 / 2 of all the furnace materials are melted, add silicon carbide. Finally, add the return materials according to the smelting situation.

[0072] S3: temperature measurement, sampling, and testing. After the charge is completely melted, the temperature is raised to a certain temperature, and then the temperature is measured, slag is removed, and sampling is performed. After the composition is adjusted to meet the requirements, the temperature is raised again. After slag removal, the power is turned off and the charge is left to stand for removal from the furnace.

[0073] S4: Spheroidizing and inoculating. 1.3% of spheroidizing agent is added to the bottom trough of the spheroidizing ladle and compacted. Then, 0.6% of the homemade Si-Ba-Ca-Sn-Sb alloy composite inoculant is added to completely cover the spheroidizing agent. Then, 3 kg of iron filings are added to completely cover the inoculant and compact it. After the spheroidizing reaction is completed, the slag is removed. Then, the molten iron is quickly poured into the prepared casting ladle. Before pouring the molten iron, 0.4% of 75 ferrosilicon alloy inoculant is placed in the casting ladle in advance. After removing the slag again, it is hoisted to the casting station.

[0074] S5: pouring. After the temperature measurement is qualified, the molten iron is poured into the sand casting mold made by the V-method process. During the pouring process, the flow is instantaneously inoculated. The amount added is about 0.1% of the amount of molten iron. The pouring is completed within a period of time after the spheroidization reaction.

[0075] S6: Maintaining pressure and boxing. After pouring, let it stand for a while, quickly adjust the negative pressure value to the minimum state, maintain the pressure for a while, turn off the negative pressure, continue to keep warm for a while and then box, you can get high-strength and high-plasticity ductile iron material.

[0076] In step S1, the mass percentage is adjusted as follows:

[0077] C:3.71, Si:2.69, Mn:0.32, Cu:0.43, P:0.05, S:0.012, RE:0.016, Mg:0.048, Sn:0.032, Sb:0.009, and the rest is Fe.

[0078] In step S1, the raw materials used in production include 08 aluminum scrap steel briquettes, recycled iron, carburizer, and silicon carbide.

[0079] In step S4, the spheroidizing inoculation process adopts Mg6RE2 spheroidizing agent, homemade Si-Ba-Ca-Sn-Sb alloy composite inoculant, ladle injection method for primary inoculation, 75 ferrosilicon alloy inverted injection method for secondary inoculation, and high-efficiency flow inoculation treatment. The required proportion of ferrite and pearlite matrix is ​​obtained by controlling Sn and Sb and adjusting Si, Mn, and Cu contents. The V casting process is adopted. After pouring, the cooling rate of the casting is controlled by adjusting the size of the negative pressure and the pressure extraction time, and the grain is refined by the unpacking time.

[0080] In step S2, the laying area of ​​the steel chips is 100 mm ± 10 mm, and when molten iron with a depth of 100 mm appears at the bottom of the furnace, the required carburizer is added.

[0081] In step S3, the first temperature rise needs to be within the range of 1410-1430°C, the adjusted second temperature rise needs to be above 1550°C, and the particle size range of the spheroidizing agent is 8-25 mm.

[0082] In step S4, the particle size of the 75 ferrosilicon alloy inoculant is in the range of 3-8 mm.

[0083] In step S5, the negative pressure value needs to be adjusted to between -0.06 MPa and -0.045 MPa before pouring.

[0084] In step S6, after pouring, the standing time is 6-8 minutes, the pressure holding time is 15 minutes, and the heat preservation time is 10 minutes.

[0085] Hardness 247HB, 254HB, tensile strength σb = 821MPa, 809MPa, yield strength σ0.2 = 446MPa, 452MPa, elongation δ = 12.5%, 11.0%. Its metallographic structure is as follows Figure 5-6 As shown: spheroidization level 2-3, ball diameter level 6-8, pearlite volume 70%.

[0086] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. Ductile iron casting process, characterized in that: The following steps are involved: S1: batching, according to the mass percentage, 60-65% of scrap steel, 35-40% of recycled materials, 2-3% of recarburizer, and 1% of silicon carbide are batched; S2: Charge and smelt. Spread a layer of steel scraps on the bottom of the furnace, add scrap steel and start electric smelting. When a certain depth of molten iron appears at the bottom of the furnace, add 40% of the required carburizer. Add the remaining carburizer gradually while melting. When 1 / 3 to 1 / 2 of all the furnace materials are melted, add silicon carbide. Finally, add the return materials according to the smelting situation. S3: temperature measurement, sampling, and testing. After the charge is completely melted, the temperature is raised to a certain temperature, and then the temperature is measured, slag is removed, and sampling is performed. After the composition is adjusted to meet the requirements, the temperature is raised again. After slag removal, the power is turned off and the charge is left to stand for removal from the furnace. S4: Spheroidizing and inoculating. 1.3% of spheroidizing agent is added to the bottom trough of the spheroidizing ladle and compacted. Then, 0.6% of the homemade Si-Ba-Ca-Sn-Sb alloy composite inoculant is added to completely cover the spheroidizing agent. Then, 3 kg of iron filings are added to completely cover the inoculant and compact it. After the spheroidizing reaction is completed, the slag is removed. Then, the molten iron is quickly poured into the prepared casting ladle. Before pouring the molten iron, 0.4% of 75 ferrosilicon alloy inoculant is placed in the casting ladle in advance. After removing the slag again, it is hoisted to the casting station. S5: pouring. After the temperature measurement is qualified, the molten iron is poured into the sand casting mold made by the V-method process. During the pouring process, the flow is instantaneously inoculated. The amount added is about 0.1% of the amount of molten iron. The pouring is completed within a period of time after the spheroidization reaction. S6: Maintaining pressure and boxing. After pouring, let it stand for a while, quickly adjust the negative pressure value to the minimum state, maintain the pressure for a while, turn off the negative pressure, continue to keep warm for a while and then box, you can get high-strength and high-plasticity ductile iron material.

2. The ductile iron casting process according to claim 1, characterized in that: In step S1, the mass percentage is adjusted as follows: C: 3.6-3.85; Si: 2.4-2.8; Mn: 0.3-0.5; P: ≤ 0.03; S: ≤ 0.02; Cu: 0.4-0.5; Sn : 0.02—0.08; Sb: 0.01—0.04; Mg: 0.04—0.06; RE: 0.015—0.04; the rest is Fe.

3. The ductile iron casting process according to claim 1, characterized in that: In step S1, the raw materials used in production include 08 aluminum scrap steel briquettes, recycled iron, carburizer, and silicon carbide.

4. The ductile iron casting process according to claim 1, characterized in that: In step S4, the spheroidizing inoculation process adopts Mg6RE2 spheroidizing agent, homemade Si-Ba-Ca-Sn-Sb alloy composite inoculant, ladle injection method for primary inoculation, 75 ferrosilicon alloy inverted injection method for secondary inoculation, and high-efficiency flow inoculation treatment. The required proportion of ferrite and pearlite matrix is ​​obtained by controlling Sn and Sb and adjusting Si, Mn, and Cu contents. The V casting process is adopted. After pouring, the cooling rate of the casting is controlled by adjusting the size of the negative pressure and the pressure extraction time, and the grain is refined by the unpacking time.

5. The ductile iron casting process according to claim 1, characterized in that: In step S2, the laying area of ​​the steel chips is 100 mm ± 10 mm, and when molten iron with a depth of 100 mm appears at the bottom of the furnace, the required carburizer is added.

6. The ductile iron casting process according to claim 1, characterized in that: In step S3, the first temperature rise needs to be within the range of 1410-1430°C, the adjusted second temperature rise needs to be above 1550°C, and the particle size range of the spheroidizing agent is 8-25 mm.

7. The ductile iron casting process according to claim 1, characterized in that: In step S4, the particle size of the 75 ferrosilicon alloy inoculant is in the range of 3-8 mm.

8. The ductile iron casting process according to claim 1, characterized in that: In step S5, the negative pressure value needs to be adjusted to between -0.06 MPa and -0.045 MPa before pouring.

9. The ductile iron casting process according to claim 1, characterized in that: In step S6, after pouring, the standing time is 6-8 minutes, the pressure holding time is 15 minutes, and the heat preservation time is 10 minutes.

Citation Information

Cited By

  • Nodular cast iron and production process

    CN120350292A

  • Ductile iron and production process

    CN120350292B