Nitralloy material and application thereof in steel

By optimizing the preparation process of nitride alloy materials and controlling the phase ratio and cooling rate, the problem of nitride alloy blocks being difficult to break was solved, the crushing efficiency and alloy utilization rate were improved, powder loss and environmental pollution were reduced, and the performance of steel was enhanced.

CN118996293APending Publication Date: 2024-11-22ANHUI ZHONGYUAN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411095730.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing nitride alloy blocks are not easily broken, resulting in low alloy utilization, large powder loss, serious environmental pollution, and unstable steel performance strengthening effect.

Method used

By controlling the preparation process of nitride alloy materials and ensuring the ratio of silicon nitride and vanadium nitride phases and the cooling rate, nitride alloy blocks with good crushing performance are prepared, including the proportion of α-Si3N4 and β-Si3N4 phases, as well as the proportion of VN, V2N, and V3N phases, with the cooling rate controlled at 3-5℃/s.

Benefits of technology

It improves the crushing efficiency of nitride alloy blocks, reduces powder loss, reduces dust, enhances the meltability and effective utilization of the alloy in molten steel, and improves the performance of steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996293A_ABST
    Figure CN118996293A_ABST
Patent Text Reader

Abstract

The invention discloses a nitroalloy material and application thereof in steel. The nitride alloy material comprises nitride or nitride alloy of one or more elements and must comprise silicon nitride, phases of the silicon nitride separated out in the nitride alloy material comprise alpha-Si3N4 and beta-Si3N4 phases, the proportion of the alpha-Si3N4 phase is 79-96 wt%, and the proportion of the beta-Si3N4 phase is 4-21 wt%. The alloy material has some defective phases inside, so that the alloy material has better crushing performance, the crushing efficiency is improved, the proportion of powder is reduced, the loss of raw materials is reduced, flying dust on site is avoided, and the environmental quality is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nitrided alloy materials, and more specifically, relates to a nitrided alloy material and its application in steel. Background Art

[0002] Nitriding alloy is an alloy widely used in the process of steel smelting. In today's steel production, in order to improve the strength of steel, it is necessary to add alloys such as ferrovanadium or ferroniobium during the steelmaking process to achieve this effect through microalloying. In order to give full play to the microalloying strengthening effect of vanadium and niobium, it is generally necessary to add an appropriate amount of nitriding alloy during steelmaking to form strong carbonitrides with microalloying elements niobium and vanadium, thereby improving the precipitation strengthening and precipitation strengthening effects of microalloying elements. Therefore, nitriding alloys are widely used in steel smelting. At present, nitride alloys are all generated by the reaction of a single element with nitrogen, such as vanadium nitride, silicon nitride, manganese nitride, titanium nitride, chromium nitride, boron nitride, niobium nitride and other nitride alloys. In metallurgy, when producing steels with special performance requirements such as high strength, wear resistance and corrosion resistance, molten steel micro-alloying technology is usually used. For example, when producing high-strength corrosion-resistant steel, some single-element nitride alloys are usually added under appropriate steelmaking processes. However, the above method has the following prominent problems: 1) low effective utilization rate of alloys, 2) the addition time, addition order and addition amount ratio of multiple varieties of single-element nitride alloys put forward stringent requirements on the design and implementation of steelmaking processes, 3) the strengthening effect on steel properties is insufficient and unstable, and 4) the cost of use is high.

[0003] There are three main methods for vanadium-nitrogen microalloying: 1) adding vanadium-nitrogen alloy; 2) adding ferrovanadium and adding nitrogen-increasing agents (such as silicon-nitrogen alloy) during the smelting process; 3) adding ferrovanadium and blowing nitrogen or adding nitriding alloy during the smelting process.

[0004] Among them, the cored wire technology is a technical method for adding nitride alloys into molten steel. Its use process is to first crush the various additive raw materials to be added to the molten steel or molten iron (such as deoxidizer, desulfurizer, modifier, alloy material, etc.) into powders of a certain particle size, and then wrap it with a cold-rolled low-carbon steel (or non-ferrous metal) strip to form a composite material (i.e., cored wire) of any length. Then, with the help of a wire feeder, the cored wire of a specified length is fed into the ladle through the slag layer at a certain speed and inserted to a certain depth. As the cored wire continues to melt at a certain place, the additives wrapped by it will also be continuously melted into the molten steel or molten iron, interacting with the surrounding molten steel or molten iron, and deoxidizing, desulfurizing, micro-alloying, fine-tuning the composition, and modifying the treated molten liquid, so as to achieve the purpose of improving the performance of the treated metal and improving its cleanliness.

[0005] The 2009 dissertation "Study on the Crushing Process of Vanadium Nitride for Cored Wire" disclosed that the production process of crushing vanadium nitride to prepare core powder for cored wire encountered problems such as excessive fine powder, irregular particle shape and uneven particle size distribution of the crushed vanadium nitride core powder. This resulted in uneven feeding of the hopper during the cored wire preparation process, making the quality of the produced cored wire unstable, and ultimately affecting the effect of microalloying. In addition, in the preparation process of vanadium nitride core powder, excessive fine powder caused large loss of raw materials, resulting in waste of raw materials; and the dust on site was large, causing serious environmental pollution.

[0006] After searching, patent document 1 (CN105463287A) discloses a multi-element nitriding alloy material and its preparation method and application. The patent discloses a multi-component nitriding alloy. When applying the alloy block to the cored wire, the alloy block needs to be crushed into powder of a certain particle size (for example, 0.01-4.5 mm) for coating. However, the organizational structure of the alloy block is relatively tight, which makes the alloy block difficult to break, thereby affecting the addition of nitriding alloy by cored wire. Therefore, it is necessary to develop a nitriding alloy material that is easier to break and has less fine powder. Summary of the invention

[0007] 1. Problem to be solved

[0008] In view of the problem that the existing alloy blocks are difficult to break, one of the purposes of the present invention is to provide a nitrided alloy material, the alloy blocks of which have better crushing performance and better solubility in molten steel, thereby improving the effective utilization rate of the alloy.

[0009] A second object of the present invention is to provide an application of a nitrided alloy material in steel, wherein the steel includes but is not limited to high chromium cast iron, high-strength strip steel, non-quenched and tempered steel, high-strength H-shaped steel, high-speed tool steel, high-strength pipeline steel, V-grade threaded steel, HRB500 (E) high-strength earthquake-resistant steel, HRB400 (E) steel, HRB600 steel and Q620D steel.

[0010] 2. Technical solution

[0011] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0012] The first aspect of the present invention provides a nitrided alloy material, the nitrided alloy material includes nitrides or nitrided alloys of one or more elements, and must contain silicon nitride, the phases of silicon nitride precipitated inside the nitrided alloy material include α-Si3N4 and β-Si3N4 phases, the α-Si3N4 phase accounts for 79-96wt%, and the β-Si3N4 phase accounts for 4-21wt%. Analysis shows that the surface of α-Si3N4 whiskers is smooth, has a large number of defects, and has a large number of bifurcated whiskers; the surface of β-Si3N4 whiskers is smooth, basically defect-free, and has few bifurcated whiskers.

[0013] According to any embodiment of the first aspect of the present invention, under a vertical static pressure mode of 100 MPa, after at least 10 minutes, the nitrided alloy block is broken into particles, the particles are prism-like and pointed, and the pointed accounts for 60-95wt%. Preferably, the prism-like particles account for 10wt%, and the pointed accounts for 90wt%.

[0014] According to any embodiment of the first aspect of the present invention, the particle size of the particles exceeding 0.1 mm accounts for more than 80%.

[0015] According to any embodiment of the first aspect of the present invention, the average grain size of the silicon nitride is less than 0.2 μm.

[0016] According to any embodiment of the first aspect of the present invention, the nitride alloy material contains 13-32% nitrogen, 21-60% silicon, 0-27% vanadium, and 0-19% titanium calculated by atomic mass fraction.

[0017] According to any embodiment of the first aspect of the present invention, the nitrided alloy material further comprises B, Nb and RE elements, and the mass fractions of the elements are B: 0-6.5%, Nb: 0-7%, and RE: 0-8%.

[0018] According to any embodiment of the first aspect of the present invention, the nitride alloy material also contains vanadium nitride, and the preparation method of the nitride alloy material comprises: crushing-block pressing-nitriding treatment-cooling, wherein the cooling rate is controlled at 3-5°C / s during the cooling process, so that the phases of vanadium nitride precipitated inside the nitride alloy block include VN phase, V2N phase and V3N phase; wherein the proportion of VN phase is 65-90wt%, and the sum of V2N and V3N phases is 10-35wt%.

[0019] According to any embodiment of the first aspect of the present invention, the VN phase accounts for 65wt%, and the sum of the V2N and V3N phases accounts for 35wt%.

[0020] A second aspect of the present invention provides an application of the nitrided alloy material, wherein the nitrided alloy material can be applied to steel.

[0021] According to any embodiment of the second aspect of the present invention, the application is to use the nitrided alloy material for materials including but not limited to high chromium cast iron, high strength strip steel, non-quenched and tempered steel, high strength H-shaped steel, high speed tool steel, high strength pipeline steel, V grade threaded steel, HRB500 (E) high strength earthquake-resistant steel, HRB400 (E) steel, HRB600 steel and Q620D steel.

[0022] 3. Beneficial effects

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The nitrided alloy material of the present invention has some defective phases inside, for example, the phases of silicon nitride precipitated inside the nitrided alloy material include α-Si3N4 and β-Si3N4 phases, the α-Si3N4 phase accounts for 79-96wt%, and the β-Si3N4 phase accounts for 4-21wt%. Analysis shows that the surface of the α-Si3N4 whisker is smooth, has a large number of defects, and has a large number of bifurcated whiskers; the surface of the β-Si3N4 whisker is smooth, basically defect-free, and has few bifurcated whiskers, so that the alloy material has better crushing performance. The nitrided alloy block of the present invention is crushed into a cored wire, which not only improves the crushing efficiency while reducing the proportion of powder and reducing raw material loss, but also avoids dust on site and improves environmental quality.

[0025] (2) The present invention improves the process steps of nitriding the alloy, for example, the cooling rate is controlled to be 3-5°C / s during the cooling process, so that the phases of vanadium nitride precipitated inside the nitrided alloy block include VN phase, V2N phase and V3N phase; wherein the proportion of VN phase is 65-90wt%, and the sum of V2N and V3N phases is 10-35wt%. Furthermore, the alloy block of the material has good crushing performance;

[0026] (3) The nitrided alloy block of the present invention can also be used directly in molten steel as a nitrided alloy block. According to tests, the nitrided alloy of the present invention has good solubility in molten steel, which improves the effective utilization rate of the alloy and increases the yield rate of the existing nitrided alloy by 15-27%. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but it should be understood that these drawings are designed only for explanation purposes and are not intended to limit the scope of the present invention. In addition, unless otherwise specified, these drawings are intended only to conceptually illustrate the structural configurations described herein and are not necessarily drawn to scale.

[0028] Figure 1 This is a scanning electron microscope image of the nitrided alloy block after crushing according to Example 1 of the present invention;

[0029] Figure 2 This is a physical picture of the nitride alloy compact according to Example 1 of the present invention;

[0030] Figure 3 This is a physical picture of the nitrided alloy block of Example 1 of the present invention;

[0031] Figure 4 This is a physical picture of the nitrided alloy block after being crushed according to Example 1 of the present invention;

[0032] Figure 5 This is a real picture of the load-bearing mold subjected to nitriding treatment according to the present invention. DETAILED DESCRIPTION

[0033] The present disclosure may be more easily understood by reference to the following description in conjunction with the accompanying drawings and examples, all of which constitute a part of the present disclosure. It should be understood that the present disclosure is not limited to the specific products, methods, conditions or parameters described and / or shown herein. Further, the terms used herein are only used for the purpose of describing specific embodiments by way of example and are not intended to be limiting unless otherwise stated.

[0034] It should also be understood that, for the sake of clarity, certain features of the present disclosure may be described herein in the context of separate embodiments, but may also be provided in combination with each other in a single embodiment. That is, unless clearly incompatible or specifically not included, each separate embodiment is considered to be combinable with any other embodiment, and the combination is considered to represent another different embodiment. Conversely, for the sake of simplicity, the various features of the present disclosure described in the context of a single embodiment may also be provided individually or in any sub-combination. Finally, although a particular embodiment may be described as part of a series of steps or part of a more general structure, each step or substructure itself may also be considered to be an independent embodiment.

[0035] Unless otherwise indicated, it should be understood that each individual element in a list and each combination of individual elements in the list will be interpreted as a different embodiment. For example, a list of embodiments represented as "A, B, or C" should be interpreted to include embodiments "A", "B", "C", "A or B", "A or C", "B or C", or "A, B, or C".

[0036] In the present disclosure, the singular forms of the articles "a," "an," and "the" also include the corresponding plural references, and a reference to a specific value includes at least that specific value unless the context clearly indicates otherwise. Thus, for example, a reference to "a substance" is a reference to at least one of that substance and equivalents thereof.

[0037] The terms including ordinal numbers such as "first" and "second" can be used to explain various components or fluids, but these components and fluids are not limited by these terms. Therefore, without departing from the teachings of the present disclosure, these terms are only used to distinguish the component / fluid from another component / fluid.

[0038] When items are described by using the conjunction terms "... and / or...," etc., the description should be understood to include any one of the associated listed items and all combinations of one or more thereof.

[0039] In general, the use of the term "about" indicates an approximate value that may vary depending on the desired properties obtained by the disclosed subject matter, and will be interpreted in a context-dependent manner based on function. Therefore, one of ordinary skill in the art will be able to interpret a certain degree of difference on a case-by-case basis. In some cases, the number of significant figures used when expressing a particular value can be a representative technique for determining the difference allowed by the term "about". In other cases, a gradient in a range of values ​​can be used to determine the range of differences allowed by the term "about". Further, all ranges in this disclosure are inclusive and combinable, and reference to the values ​​stated in the range includes each value within the range.

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the terms used herein and / or include any and all combinations of one or more of the associated listed items.

[0041] The present invention is further described below in conjunction with specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. The essential characteristics and remarkable effects of the present invention can be reflected from the following examples, and the described embodiments are part of the embodiments of the present invention, rather than all the embodiments, and therefore, they do not limit the present invention in any way, and those skilled in the art make some non-essential improvements and adjustments based on the content of the present invention, which all belong to the protection scope of the present invention.

[0042]

Nitride alloy materials

[0043] The nitride alloy material of the present invention includes nitrides or nitride alloys of one or more elements, wherein the nitrides include but are not limited to silicon nitride, vanadium nitride, titanium nitride, etc., and must contain silicon nitride. The preparation method of the nitride alloy material includes: crushing-briquetting-nitriding treatment-cooling. The specific steps are crushing and grinding the raw material particles to a certain particle size, then using a ball press to briquette, sending them into a nitriding furnace for nitriding treatment, and finally cooling to obtain a nitride alloy block.

[0044] The above-mentioned nitriding treatment, for example, is feasible in steps of: first heating to 900-1000°C and keeping it for 3-4 hours, then heating to 1150-1200°C and keeping it for 9-10 hours, then heating to 1300-1350°C and keeping it for 6-8 hours, until heating to 1450-1900°C and keeping it for 10-12 hours. It should be noted that according to theoretical research, increasing the temperature is conducive to improving the conversion rate of the crystal, and the product coexists with α and β phases at 1400°C, and only β phase at 1850°C.

[0045] In addition, it can be seen that the temperature of the nitriding treatment is relatively high, even reaching the sintering temperature of some raw materials. However, small particle size and / or low binder phase content will lead to higher hardness while also reducing the internal porosity of the alloy block. Therefore, it is necessary to optimize the particle size and binder phase content to achieve the best sinterability, so that the alloy block of this material has better crushing performance.

[0046] The inventors surprisingly found that the phases of silicon nitride precipitated inside the nitride alloy material include α-Si3N4 and β-Si3N4 phases, the α-Si3N4 phase accounts for 79-96wt%, and the β-Si3N4 phase accounts for 4-21wt%. Analysis shows that the surface of α-Si3N4 whiskers is smooth, with a large number of defects, and a large number of bifurcated whiskers; the surface of β-Si3N4 whiskers is smooth, basically defect-free, and has few bifurcated whiskers.

[0047] Furthermore, during the cooling process, the cooling rate is controlled to be 3-5°C / s, so that the phases of vanadium nitride precipitated inside the nitrided alloy block include VN phase, V2N phase and V3N phase; wherein the VN phase accounts for 65-90wt%, and the sum of the V2N and V3N phases accounts for 10-35wt%; at the same time, it also ensures that the alloy block is not cracked as much as possible during the cooling process.

[0048] Under the premise of controlling the relative proportion of fine powder (generally controlling fine powder less than 0.01mm at 3-5wt%), from the above analysis of the internal structure, it can be seen that the possible reason is that by changing the cooling rate during the cooling process, the impurity dispersion in the internal structure of vanadium nitride is reduced and / or uniformized, so that there are a reasonable number of impurity gaps between the vanadium nitride crystals at the microscopic level. Under the action of external force, these parts can be easily fractured and broken, thereby improving the crushing efficiency; in addition, the crystal morphology of the internal vanadium nitride crystals is relatively regular, and the mutual connection method is single, which also makes the final crushed powder morphology relatively regular and the particle size distribution uniform.

[0049] It should be noted that in the prior art, the content of crushed vanadium nitride powder below 0.1mm reaches 70% (resulting in more than 5% of fine powder less than 0.01mm), which is not conducive to the preparation of cored wires on the one hand, and on the other hand, due to excessive fine powder, there is a lot of dust on site, resulting in a large loss of vanadium nitride raw materials. According to the final statistics of each batch of production on site, the loss rate of vanadium nitride crushed by the impact crusher reaches about 3%, the loss is relatively serious, and it also causes great pollution to the factory environment. In comparison, the particles of the present invention are uniform and the particle size distribution is reasonable enough. For example, the powder with a particle size less than 0.01mm accounts for 1.5%, 0.01mm-0.1mm accounts for 16.5%, and 0.1mm-5.5mm accounts for 82%, and the total proportion is calculated as 100%.

[0050] In addition, through a large number of experimental analyses, it was found that when the cooling rate was controlled to be less than 3°C / s during the cooling process, the alloy block was prone to adhesion to the nitriding mold (the particles were added to the graphite mold for nitriding treatment, such as Figure 5 When the cooling rate is controlled to be greater than 5°C / s during the cooling process, pits or grooves are easily formed on the surface of the alloy block, which is not conducive to moisture prevention.

[0051] The nitrided alloy material of the present invention meets at least one of the following requirements:

[0052] 1) The particle size of the particles exceeds 0.1 mm, accounting for more than 80%;

[0053] 2) The average grain size of the silicon nitride is less than 0.2 μm; preferably 0.1-0.2 μm;

[0054] 3) The nitride alloy material contains 13-32% nitrogen, 21-60% silicon, 0-27% vanadium and 0-19% titanium in terms of atomic mass fraction.

[0055] Furthermore, the nitrided alloy material also includes B, Nb and RE elements, and the mass fractions of the elements are B: 0-6.5%, Nb: 0-7%, and RE: 0-8%.

[0056] 4) The proportion of the VN phase is 65-90wt%, and the sum of the V2N and V3N phases is 10-35wt%; preferably, the proportion of the VN phase is 65wt%, and the sum of the V2N and V3N phases is 35wt%. There is no set requirement for the mixing ratio between the V2N and V3N phases, and they can be mixed in any ratio.

[0057] 5) The nitride alloy material comprises, calculated by atomic mass fraction; as mentioned above, the nitride alloy material comprises nitrides or nitride alloys of one or more elements, and must contain silicon nitride. Thus, the nitride alloy of the present invention may contain vanadium nitride + silicon nitride, or vanadium nitride + silicon nitride + titanium nitride, or silicon nitride + titanium nitride.

[0058]

Nitride alloy material testing method

[0059] 1. Detection of silicon nitride, vanadium nitride and nitrides

[0060] The standards involved in the content detection include: (1) GB / T 20567-2020 "Vanadium Nitrogen Alloy"; (2) GB / T24583.1-2019 "Vanadium Nitrogen Alloy - Determination of Vanadium Content - Ammonium Ferrous Sulfate Titration Method"; (3) GB / T 24583.2-2019 "Vanadium Nitrogen Alloy - Determination of Nitrogen Content - Inert Gas Melting Thermal Conductivity Method"; (4) GB / T 24583.8-2019 "Vanadium Nitrogen Alloy - Determination of Silicon, Manganese, Phosphorus and Aluminum Content - Inductively Coupled Plasma Atomic Emission Spectrometry"; (5) GB / T 37258-2018 "Silicon Nitride Ceramic Powder".

[0061] 2. Phase detection of silicon nitride and vanadium nitride

[0062] For the nitride alloy material of the present invention, the X-ray diffractometer is used for phase qualitative analysis and quantitative analysis. Through phase qualitative analysis, the measured lattice plane spacing and diffraction intensity of the material are compared with the diffraction data of the standard phase to determine the phases present in the material; according to the intensity of the diffraction pattern, the content of each phase in the material is determined.

[0063] 3. Physical testing of nitrided alloys

[0064] For the nitride alloy material of the present invention, its crushability needs to be tested. For example, the method adopted by the present invention is: under a vertical static pressure mode of 100 MPa, after at least 10 minutes, the nitride alloy block is crushed, and the particles are prism-like (having a spherical surface + an angular surface) and pointed-angled, among which the pointed-angled accounts for 60-95wt%.

[0065]

Application of nitride alloy materials

[0066] The nitrided alloy material of the present invention can be crushed to make cored wire for use in steel, or can be directly used as alloy block for use in steel; in addition, the alloy block can also be used in other fields, such as metallurgical refractory materials.

[0067] When the alloy block of the present invention is used directly, the alloy block needs to be transported. The inventor was surprised to find that the alloy block obtained by the present invention is not easy to break during transportation, and the alloy block maintains a good block shape, which can reduce the decomposition rate of the alloy block. Although the present invention hopes to obtain an easily broken alloy block (made into a cored wire), it is not desired to be easily broken when using the alloy block. However, the two are not contradictory. The titanium element in the alloy block reacts with a small amount of silicon dioxide and aluminum oxide in the raw material to form a tight network structure, which improves the compressive performance of the alloy block. The compressive strength is above 14Mpa. The external force received by the alloy block during transportation is mainly the extrusion force and friction force of the materials at the junction. The effect of these external forces is small and cannot reach the value of the compressive strength. When broken, for example, the lateral and longitudinal pressures far exceed 14MPa or more, first breaking the bonding force of the network structure, and then using the gaps between the silicon nitride crystals to break.

[0068] The above-mentioned application in steel is to use the nitrided alloy material in including but not limited to high chromium cast iron, high-strength strip steel, non-quenched and tempered steel, high-strength H-shaped steel, high-speed tool steel, high-strength pipeline steel, V-grade threaded steel, HRB500 (E) high-strength earthquake-resistant steel, HRB400 (E) steel and Q620D steel.

[0069] Example 1

[0070] Combination Figures 1 to 4 As shown, the preparation method of the nitride alloy material of this embodiment comprises the following steps:

[0071] Step S1, selecting raw materials: ferrovanadium, vanadium pentoxide, vanadium-containing slag, ferrosilicon, metallic silicon, ferroboron, and ferroniobium. The raw materials and reagents used in the present invention, unless otherwise specified, are all purchased from commercial sources;

[0072] Step S2, crushing the materials selected in step S1 respectively, and then grinding them to a particle size of 120-600 mesh, and the grinding can be carried out by a ball mill or the like;

[0073] Step S3, the raw material fine powders obtained in step S2 are proportioned, and then a binder accounting for 2% by mass of the total raw material fine powder and 5% of graphite carbon are added, mixed and pressed into blocks using a strong ball press at a pressure of 120 MPa; the binder is sodium polystyrene sulfonate and / or polyacrylamide; the mass ratio of sodium polystyrene sulfonate and polyacrylamide can be 1:1; sodium polystyrene sulfonate and polyacrylamide can play an adhesion role at room temperature, which is convenient for molding; at a temperature of 450°C, sodium polystyrene sulfonate and polyacrylamide can be decomposed and will not be brought into the nitrided alloy block;

[0074] Although sodium polystyrene sulfonate and / or polyacrylamide mainly play a homogenizing role, they also play a role in coating the raw material particles (such as ferrovanadium particles). Through observation and research on the appearance of the raw material particles, some component particles have exposed surfaces (part of the reaction particles are exposed due to external forces). Sodium polystyrene sulfonate and / or polyacrylamide adhere to these exposed surfaces and can connect other raw material particles with these particles as much as possible, shorten the spatial distance between each other, and promote the rapid reaction of the raw materials.

[0075] Step S4, placing the compact obtained in step S3 into a pretreatment furnace (e.g., a vacuum furnace), heating it to 700°C for insulation, and filling the furnace with protective gas (argon-nitrogen mixed gas, wherein the purity of Ar gas is 99% and the purity of N2 is 98%), and pretreating for 4 hours;

[0076] Step S5, placing the pretreated pressed block into a nitriding furnace for nitriding treatment, introducing nitrogen during the nitriding treatment, with a pressure of 0.15 MPa, first heating to 900°C for 3 hours, then heating to 1150°C for 10 hours, and then heating to 1350°C for 7 hours, until heating to 1500°C for 11 hours;

[0077] Step S6, after the nitriding treatment is completed, slowly cool to below 300°C in the furnace, and control the cooling rate to 5°C / s during the cooling process, so that the nitrided alloy block is precipitated: the silicon nitride phase precipitated in the nitrided alloy material includes α-Si3N4 and β-Si3N4 phases, and the vanadium nitride phase precipitated in the nitrided alloy material includes VN phase, V2N phase and V3N phase; then take out of the furnace and cool to room temperature to obtain a multi-element nitrided alloy with a particle size of 3-70mm.

[0078]

Nitride alloy material testing method

[0079] 1. The nitride alloy material of the present invention adopts X-ray diffractometer phase qualitative analysis and quantitative analysis. Through phase qualitative analysis, the measured lattice plane spacing and diffraction intensity of the material are compared with the diffraction data of the standard phase to determine the phases present in the material; according to the intensity of the diffraction pattern, the content of each phase in the material is determined; silicon nitride, vanadium nitride and other nitrides are measured respectively, and the diffraction peaks of silicon nitride and vanadium nitride appear in the RXD diagram, thereby determining that the alloy block contains vanadium nitride and silicon nitride.

[0080] After testing, it was found that the phases of silicon nitride included α-Si3N4 and β-Si3N4 phases, the α-Si3N4 phase accounted for 90wt% and the β-Si3N4 phase accounted for 10wt%.

[0081] The proportion of the VN phase is 70wt%, and the sum of the V2N and V3N phases is 30wt%. There is no set requirement for the mixing ratio between the V2N and V3N phases, and they can be mixed in any ratio.

[0082] 2. According to the standards: (1) GB / T 20567-2020 "Vanadium-Nitrogen Alloy"; (2) GB / T 24583.1-2019 "Vanadium-Nitrogen Alloy - Determination of Vanadium Content - Ammonium Ferrous Sulfate Titration Method"; (3) GB / T 24583.2-2019 "Vanadium-Nitrogen Alloy - Determination of Nitrogen Content - Inert Gas Melting Thermal Conductivity Method"; (4) GB / T 24583.8-2019 "Vanadium-Nitrogen Alloy - Determination of Silicon, Manganese, Phosphorus and Aluminum Content - Inductively Coupled Plasma Atomic Emission Spectrometry"; (5) GB / T 37258-2018 "Silicon Nitride Ceramic Powder", obtain the specific contents of silicon nitride, vanadium nitride and other nitrides.

[0083] 3. Physical testing of nitrided alloys

[0084] For the nitride alloy material of the present invention, its crushability needs to be tested. For example, the method adopted by the present invention is: under a vertical static pressure mode of 100 MPa, the nitride alloy block is crushed after at least 10 minutes, and after screening, the particles are prism-like and pointed-angled.

[0085] 1) If Figure 1 As shown, the obtained nitrided alloy block was subjected to a vertical static pressure mode of 100 MPa for 10 minutes, and the nitrided alloy block was broken into particles, wherein the particles were prismatic in shape accounting for 10wt%, and the particles were pointed in shape accounting for 90wt%. The composition of the particles after final crushing was analyzed, and it was obtained that the powder with a particle size of 0.01mm-5.5mm accounted for 98.5%, the powder with a particle size less than 0.01mm accounted for about 1.5%, and there was a small amount of large particles.

[0086] 2) The obtained nitrided alloy block is directly used in molten steel. By observing that it has good solubility in molten steel, the decomposition rate of the alloy block is reduced, and the nitrogen recovery rate is effectively improved.

[0087] Example 2

[0088] The preparation method of the nitrided alloy material of this embodiment comprises the following steps:

[0089] Step S1, selecting raw materials: ferrovanadium, vanadium pentoxide, vanadium-containing slag, ferrosilicon, metallic silicon, ferroboron, and ferroniobium. The raw materials and reagents used in the present invention, unless otherwise specified, are all purchased from commercial sources;

[0090] Step S2, crushing the materials selected in step S1 respectively, and then grinding them to a particle size of 120-600 mesh;

[0091] Step S3, the raw material fine powders obtained in step S2 are proportioned, and then 3% of the binder and 4% of graphite are added to the total raw material fine powder, mixed and pressed into blocks using a strong ball press at a pressure of 110 MPa; the binder is sodium polystyrene sulfonate and polyacrylamide;

[0092] Step S4, placing the pressed blocks obtained in step S3 into a pretreatment furnace, heating them to 750°C for insulation, and filling the furnace with protective gas for pretreatment for 5 hours;

[0093] Step S5, placing the pretreated pressed block into a nitriding furnace for nitriding treatment, introducing nitrogen during the nitriding treatment, with a pressure of 0.18 MPa, first heating to 1000° C. for 4 hours, then heating to 1150° C. for 9 hours, and then heating to 1300° C. for 8 hours, until heating to 1450° C. for 12 hours;

[0094] Step S6, after the nitriding treatment is completed, slowly cool to below 300°C in the furnace, and control the cooling rate to 3°C / s during the cooling process, so that the nitrided alloy block is precipitated: the silicon nitride phase precipitated in the nitrided alloy material includes α-Si3N4 and β-Si3N4 phases, and the vanadium nitride phase precipitated in the nitrided alloy material includes VN phase, V2N phase and V3N phase; then take out of the furnace and cool to room temperature to obtain a multi-element nitrided alloy with a particle size of 3-70mm.

[0095]

Nitride alloy material testing method

[0096] 1. The nitride alloy material of the present invention adopts X-ray diffractometer phase qualitative analysis and quantitative analysis. Through phase qualitative analysis, the measured lattice plane spacing and diffraction intensity of the material are compared with the diffraction data of the standard phase to determine the phases present in the material; according to the intensity of the diffraction pattern, the content of each phase in the material is determined; silicon nitride, vanadium nitride and other nitrides are measured respectively, and the diffraction peaks of silicon nitride and vanadium nitride appear in the RXD diagram, thereby determining that the alloy block contains vanadium nitride and silicon nitride.

[0097] After testing, it was found that the phases of silicon nitride included α-Si3N4 and β-Si3N4 phases, the α-Si3N4 phase accounted for 89wt% and the β-Si3N4 phase accounted for 11wt%.

[0098] The proportion of the VN phase is 86wt%, and the sum of the V2N and V3N phases is 14wt%. There is no requirement for the mixing ratio between the V2N and V3N phases, and they can be mixed in any ratio.

[0099] 2. According to the standards: (1) GB / T 20567-2020 "Vanadium-Nitrogen Alloy"; (2) GB / T 24583.1-2019 "Vanadium-Nitrogen Alloy - Determination of Vanadium Content - Ammonium Ferrous Sulfate Titration Method"; (3) GB / T 24583.2-2019 "Vanadium-Nitrogen Alloy - Determination of Nitrogen Content - Inert Gas Melting Thermal Conductivity Method"; (4) GB / T 24583.8-2019 "Vanadium-Nitrogen Alloy - Determination of Silicon, Manganese, Phosphorus and Aluminum Content - Inductively Coupled Plasma Atomic Emission Spectrometry"; (5) GB / T 37258-2018 "Silicon Nitride Ceramic Powder", obtain the specific contents of silicon nitride, vanadium nitride and other nitrides.

[0100] 3. Physical testing of nitrided alloys

[0101] For the nitride alloy material of the present invention, its crushability needs to be tested. For example, the method adopted by the present invention is: under a vertical static pressure mode of 100 MPa, the nitride alloy block is crushed after at least 10 minutes, and after screening, the particles are prism-like and pointed-angled.

[0102] The obtained nitrided alloy block was subjected to a vertical static pressure mode of 100 MPa for 12 minutes, and the nitrided alloy block was broken into particles, wherein the prism-shaped particles accounted for 13wt% and the pointed-angle-shaped particles accounted for 87wt%.

[0103] In the same period of time, the final crushed particle composition was analyzed, and it was found that the powder with a particle size of 0.01mm-5.5mm accounted for 98.6%, the powder with a particle size less than 0.01mm accounted for about 1.4%, and a small amount of large particles; while the crushed particle composition of the prior art was 93.5% of the powder with a particle size of 0.01mm-5.5mm, the powder with a particle size less than 0.01mm accounted for about 6.5%, and a small amount of large particles. Therefore, the crushing efficiency of the present invention is effectively improved, while reducing the proportion of powder, reducing raw material loss, avoiding dust on site, and improving environmental quality.

[0104] Example 3

[0105] The preparation method of the nitrided alloy material of this embodiment comprises the following steps:

[0106] Step S1, selecting raw materials: ferrovanadium, vanadium pentoxide, vanadium-containing slag, ferrosilicon, metallic silicon, ferroboron, and ferroniobium. The raw materials and reagents used in the present invention, unless otherwise specified, are all purchased from commercial sources;

[0107] Step S2, crushing the materials selected in step S1 respectively, and then grinding them to a particle size of 120-600 mesh;

[0108] Step S3, mixing the raw material fine powders obtained in step S2 in proportion, then adding 2.5% of the binder and 5% of graphite carbon accounting for the mass fraction of the total raw material fine powder, mixing and briquetting with a strong ball press at a pressure of 100 MPa; the binder is sodium polystyrene sulfonate and polyacrylamide;

[0109] Step S4, placing the pressed blocks obtained in step S3 into a pretreatment furnace, heating them to 750°C for insulation, and filling the furnace with protective gas for pretreatment for 3 hours;

[0110] Step S5, placing the pretreated pressed block into a nitriding furnace for nitriding treatment, introducing nitrogen during the nitriding treatment, with a pressure of 0.15 MPa, first heating to 1000°C for 4 hours, then heating to 1200°C for 10 hours, and then heating to 1300°C for 6 hours, until heating to 1530°C for 12 hours;

[0111] Step S6, after the nitriding treatment is completed, slowly cool to below 300°C in the furnace, and control the cooling rate to 3°C / s during the cooling process, so that the nitrided alloy block is precipitated: the silicon nitride phase precipitated in the nitrided alloy material includes α-Si3N4 and β-Si3N4 phases, and the vanadium nitride phase precipitated in the nitrided alloy material includes VN phase, V2N phase and V3N phase; then take out of the furnace and cool to room temperature to obtain a multi-element nitrided alloy with a particle size of 3-70mm.

[0112]

Nitride alloy material testing method

[0113] 1. The nitride alloy material of the present invention adopts X-ray diffractometer phase qualitative analysis and quantitative analysis. Through phase qualitative analysis, the measured lattice plane spacing and diffraction intensity of the material are compared with the diffraction data of the standard phase to determine the phases present in the material; according to the intensity of the diffraction pattern, the content of each phase in the material is determined; silicon nitride, vanadium nitride and other nitrides are measured respectively, and the diffraction peaks of silicon nitride and vanadium nitride appear in the RXD diagram, thereby determining that the alloy block contains vanadium nitride and silicon nitride.

[0114] After testing, it was found that the phases of silicon nitride included α-Si3N4 and β-Si3N4 phases, the α-Si3N4 phase accounted for 85wt%, and the β-Si3N4 phase accounted for 15wt%.

[0115] The proportion of the VN phase is 89wt%, and the sum of the V2N and V3N phases is 11wt%. There is no set requirement for the mixing ratio between the V2N and V3N phases, and they can be mixed in any ratio.

[0116] 2. According to the standards: (1) GB / T 20567-2020 "Vanadium-Nitrogen Alloy"; (2) GB / T 24583.1-2019 "Vanadium-Nitrogen Alloy - Determination of Vanadium Content - Ammonium Ferrous Sulfate Titration Method"; (3) GB / T 24583.2-2019 "Vanadium-Nitrogen Alloy - Determination of Nitrogen Content - Inert Gas Melting Thermal Conductivity Method"; (4) GB / T 24583.8-2019 "Vanadium-Nitrogen Alloy - Determination of Silicon, Manganese, Phosphorus and Aluminum Content - Inductively Coupled Plasma Atomic Emission Spectrometry"; (5) GB / T 37258-2018 "Silicon Nitride Ceramic Powder", obtain the specific contents of silicon nitride, vanadium nitride and other nitrides.

[0117] 3. Physical testing of nitrided alloys

[0118] For the nitride alloy material of the present invention, its crushability needs to be tested. For example, the method adopted by the present invention is: under a vertical static pressure mode of 100 MPa, the nitride alloy block is crushed after at least 10 minutes, and after screening, the particles are prism-like and pointed-angled.

[0119] The obtained nitrided alloy block was placed under a vertical static pressure mode of 100 MPa for 12 minutes, and the nitrided alloy block was broken into particles, of which the prism-shaped particles accounted for 15wt%, the pointed-angle-shaped particles accounted for 85wt%, and the final crushed particle composition was analyzed, and it was found that the powder with a particle size of 0.01mm-5.5mm accounted for 98.7%, the powder with a particle size less than 0.01mm accounted for about 1.3%, and there was a small amount of large particles.

[0120] Example 4

[0121] The preparation method of the nitrided alloy material of this embodiment comprises the following steps:

[0122] Step S1, selecting raw materials: ferrovanadium, vanadium pentoxide, vanadium-containing slag, ferrosilicon, metallic silicon, ferroboron, and ferroniobium;

[0123] Step S2, crushing the materials selected in step S1 respectively, and then grinding them to a particle size of 120-600 mesh;

[0124] Step S3, the raw material fine powders obtained in step S2 are mixed in proportion, and then a binder accounting for 2.5% by mass of the total raw material fine powder and 7% of graphite carbon are added, mixed and pressed into blocks using a strong ball press at a pressure of 110 MPa; the binder is sodium polystyrene sulfonate and polyacrylamide;

[0125] Step S4, placing the pressed blocks obtained in step S3 into a pretreatment furnace, heating them to 750°C for insulation, and filling the furnace with protective gas for pretreatment for 3 hours;

[0126] Step S5, placing the pretreated pressed block into a nitriding furnace for nitriding treatment, introducing nitrogen during the nitriding treatment, with a pressure of 0.17 MPa, first heating to 1000°C for 4 hours, then heating to 1200°C for 10 hours, and then heating to 1300°C for 6 hours, until heating to 1530°C for 12 hours;

[0127] Step S6, after the nitriding treatment is completed, slowly cool to below 300°C in the furnace, and control the cooling rate to 3°C / s during the cooling process, so that the nitrided alloy block is precipitated: the phases of silicon nitride precipitated inside the nitrided alloy material include α-Si3N4 and β-Si3N4 phases.

Claims

1. A nitride alloy material, comprising nitrides or nitride alloys of one or more elements and must contain silicon nitride, characterized in that: The phases of silicon nitride precipitated inside the nitride alloy material include α-Si3N4 and β-Si3N4 phases, wherein the α-Si3N4 phase accounts for 79-96wt% and the β-Si3N4 phase accounts for 4-21wt%.

2. The nitride alloy material according to claim 1, characterized in that: Under the vertical static pressure mode of 100 MPa, after at least 10 minutes, the nitride alloy block was broken into particles, the shapes of which were prism-like and pointed-angle-like, of which the pointed-angle-shaped particles accounted for 60-95wt%.

3. The nitride alloy material according to claim 2, characterized in that: The prism-shaped particles account for 10wt%, and the pointed-angle-shaped particles account for 90wt%.

4. The nitride alloy material according to claim 3, characterized in that: The particle size of the particles exceeds 0.1 mm, accounting for more than 80%.

5. The nitride alloy material according to claim 4, characterized in that: The average grain size of silicon nitride is less than 0.2 μm.

6. The nitride alloy material according to any one of claims 1 to 5, characterized in that: The nitride alloy material contains 13-32% of nitrogen element, 21-60% of silicon element, 0-27% of vanadium element, and 0-19% of titanium element according to atomic mass fraction.

7. The nitride alloy material according to claim 6, characterized in that: The nitrided alloy material also includes B, Nb and RE elements according to the mass fraction, and the mass fraction of each element is B: 0-6.5%, Nb: 0-7%, RE: 0-8%.

8. The nitride alloy material according to claim 1, characterized in that: It also contains vanadium nitride, and the phases of vanadium nitride precipitated inside the nitride alloy material include VN phase, V2N phase and V3N phase; the VN phase accounts for 65-90wt%, and the sum of the V2N and V3N phases accounts for 10-35wt%.

9. The nitride alloy material according to claim 8, characterized in that: The VN phase accounts for 65wt%, and the sum of the V2N and V3N phases accounts for 35wt%.

10. An application of the nitrided alloy material according to claims 1 to 9 in steel, wherein the steel includes but is not limited to high chromium cast iron, high strength strip steel, non-quenched and tempered steel, high strength H-shaped steel, high speed tool steel, high strength pipeline steel, V-grade threaded steel, HRB500 (E) high strength earthquake-resistant steel, HRB400 (E) steel, HRB600 steel and Q620D steel.