Method for increasing thickness of heat treatment QPQ compound layer
By using non-ionic surfactant and ultrasonic cleaning solution of modified silica in QPQ technology, combined with mechanical oil removal and shot peening, the problem of workpiece surface pollution affecting nitriding effect is solved, and the wear resistance of workpieces is improved and corrosion resistance, and achieve environmentally friendly and easy-to-recycle cleaning liquid use.
Patent Information
- Application Number
- CN202411116089.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
The existing QPQ technology cannot completely remove surface contaminants during workpiece cleaning, affecting the nitriding effect and subsequent treatment, resulting in poor material wear resistance, corrosion resistance and strength.
Ultrasonic cleaning methods containing non-ionic surfactants, modified silica and specific cleaning liquid are adopted, combined with mechanical oil removal and shot peening to ensure that the surface of the workpiece is cleaned and nitriding and oxidizing to form a thick protective layer.
It significantly improves the hardness and wear resistance of the surface compound layer of the workpiece, enhances corrosion resistance, and the cleaning liquid is environmentally friendly and easy to recycle, suitable for large-scale production.
Smart Images

Figure BDA0004993660470000101 
Figure BDA0004993660470000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal surface treatment, and in particular relates to a method for increasing the thickness of a heat-treated QPQ compound layer. Background Art
[0002] The essence of QPQ (Quench-Polish-Quench) technology is low-temperature salt bath nitriding + salt bath oxidation or low-temperature salt bath nitrocarburizing + salt bath oxidation. It is a metal parts surface modification technology with the advantages of high corrosion resistance, high wear resistance and micro deformation. The surface of the workpiece treated by QPQ technology is Fe3O4 oxide film, and its corrosion resistance is much higher than the level of surface protection technologies such as chrome plating and nickel plating. Medium carbon steel can replace stainless steel in many fields after QPQ treatment. At the same time, QPQ process can replace traditional anti-corrosion processes such as blackening, phosphating and nickel plating.
[0003] At present, the high corrosion resistance of QPQ technology has attracted great attention from relevant industries, especially industries with serious corrosion problems such as petroleum and chemical industry. However, before nitriding the workpiece, it is necessary to clean, degrease, derust and remove the metal chips attached to the surface of the workpiece during machining, as well as the cooling lubricant during cutting and the residues of certain metal cleaning agents, which exist in the form of surface film on the surface of the workpiece, will hinder the absorption of nitrogen and carbon on the surface of the workpiece. At present, the workpiece is mostly washed with simple high-pressure water flow when cleaning, resulting in incomplete cleaning of the workpiece surface, which not only affects the nitriding effect, but also affects the QPQ treatment of the workpiece surface in the later stage, reduces the life of the mold, and also contaminates the solid salt and QPQ salt bath salt during the nitriding process, which brings inconvenience to the processing, makes the nitriding effect poor, and causes the material to have problems of poor wear resistance, corrosion resistance, strength and toughness. Summary of the invention
[0004] The object of the present invention is to provide a method for increasing the thickness of a heat-treated QPQ compound layer to solve one of the problems of the technology mentioned in the background art.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for increasing the thickness of a heat-treated QPQ compound layer comprises the following steps:
[0007] S1. Pretreatment: Mechanically remove oil, rust, dry and shot peen the workpiece;
[0008] S2. Pre-cleaning: Put the workpiece into an ultrasonic cleaning machine containing a cleaning solution for cleaning, and then put it into a rinsing tank for rinsing and drying; the cleaning solution includes the following raw materials in parts by weight:
[0009] 8-12 parts of nonionic surfactant, 1-3 parts of sodium silicate, 0.5-1 parts of polydimethylsiloxane, 1-3 parts of disodium ethylenediaminetetraacetic acid, 3-6 parts of modified silicon dioxide, 65-80 parts of water;
[0010] S3, preheating: put the workpiece into the preheating furnace for preheating treatment;
[0011] S4, nitriding: putting the preheated workpiece into a nitriding furnace for nitriding treatment;
[0012] S5, oxidation: After the nitrided workpiece is subjected to salt dripping treatment, it is placed in an oxidation furnace for oxidation treatment;
[0013] S6, post-cleaning: After the oxidized workpiece is subjected to salt dripping treatment, it is placed in a quenching water tank for quenching cooling, and after complete cooling, it is rinsed and blown dry;
[0014] S7, closing: closing the workpiece;
[0015] S8, inspection and packaging: Inspect the workpieces, and the processing is completed after passing the quality inspection.
[0016] Furthermore, the nonionic surfactant in S2 is at least one of fatty alcohol polyoxyethylene ether, octylphenol polyoxyethylene ether and nonylphenol polyoxyethylene ether. Compared with other surfactants, nonionic surfactants do not have charged free radicals, can interact with water molecules through hydrogen bonds, and have excellent stability in water.
[0017] Furthermore, the modified silicon dioxide is prepared by the following steps:
[0018] Silicon dioxide is added to deionized water, ultrasonically dispersed and stirred, sodium alginate is added, stirred for reaction, and then freeze-dried and immersed in a calcium chloride solution, stirred for reaction, washed and dried to obtain modified silicon dioxide. In the above technical scheme, modified silicon dioxide is prepared by porous sodium alginate and porous silicon dioxide under the conditions of freeze drying and calcium ion cross-linking, and the adsorption of sodium alginate and silicon dioxide is exerted at the same time, and various oils and solid particles in the solution can be greatly adsorbed, and pollutants such as oil are quickly adsorbed in the pores, with excellent adsorption capacity. At the same time, the prepared modified silicon dioxide material is porous, can be suspended in a solvent, and is easy to recycle and can be used repeatedly.
[0019] Furthermore, the usage ratio of silicon dioxide, deionized water, sodium alginate and calcium chloride solution is 0.3-0.5 g: 25 mL: 1 g: 40 mL.
[0020] Furthermore, the preparation method of the cleaning liquid is as follows: nonionic surfactant, sodium silicate, polydimethylsiloxane, disodium ethylenediaminetetraacetic acid, modified silicon dioxide and water are mixed according to weight parts to obtain the cleaning liquid.
[0021] Furthermore, the temperature in the ultrasonic cleaning machine in S2 is 60-70° C., and the cleaning time is 8-10 min.
[0022] Furthermore, the ultrasonic cleaning machine in S2 replaces the cleaning liquid once every 40 furnaces of cleaning.
[0023] Furthermore, the S2 rinsing method is: introducing compressed air, entering a primary rinsing tank for rinsing with clean water for 5-8 minutes, and then entering a secondary rinsing tank for rinsing with clean water for 2-3 minutes.
[0024] Furthermore, the preheating temperature in S3 is 360±10°C, and the preheating time is 180-200min.
[0025] Furthermore, in S4, the nitriding temperature is 490±10° C., and the nitriding time is 480-500 min.
[0026] Furthermore, a nitriding salt is used in the S4 nitriding furnace for nitriding reaction, wherein the nitriding salt is a cyanate-type base salt, wherein the cyanate concentration is 32%-39%.
[0027] Furthermore, in S5, the oxidation temperature is 400±10°C, and the oxidation time is 15-20min.
[0028] Furthermore, the specific method of rinsing in S6 is: introducing compressed air, entering the first rinsing tank for rinsing with clean water for 10-15 minutes, and then entering the second rinsing tank for rinsing with clean water for 1-5 minutes.
[0029] Furthermore, in S6, the water in the quenching water tank is changed once every 20 heats, the water in the first rinsing tank is changed once every 60 heats, and the water in the second rinsing tank is changed once every 80 heats.
[0030] Beneficial effects of the present invention:
[0031] The present invention provides a method for increasing the thickness of a heat-treated QPQ compound layer. First, the workpiece material is pre-cleaned, and the self-made cleaning liquid of the present invention is used in an ultrasonic cleaning machine. The cleaning liquid has excellent cleaning ability for organic matter and aqueous substances on the surface of the metal workpiece, and effectively removes particles, inorganic salts, metal pollutants and organic pollutants on the surface of the workpiece material. Then, the workpiece material is placed in a nitriding furnace and reacted with a cyanate-type base salt to undergo a nitriding reaction. After the nitriding treatment, the active single atoms in the salt bath continuously diffuse to the surface of the workpiece, penetrate into the interior of the workpiece, and finally form a thicker protective layer, thereby improving the surface performance of the workpiece and greatly improving the hardness, wear resistance and corrosion resistance of the surface compound layer of the workpiece material.
[0032] Furthermore, the cleaning liquid prepared in the present invention does not contain phosphorus in its formula, and after use, the discharged sewage has little impact on the environment, which can effectively protect the environment, and the cleaning liquid has a strong cleaning ability for oil stains, etc., and can clean up oil stains and dirt on the surface of the workpiece, which is helpful for subsequent processing procedures and improves the hardness, wear resistance and corrosion resistance of the surface protective layer of the workpiece after heat treatment QPQ. At the same time, the prepared modified silicon dioxide is simple to prepare, green and low-cost, and is easy to separate and recycle, and can be recycled for many times, which is suitable for large-scale production applications. DETAILED DESCRIPTION
[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] This embodiment provides a cleaning solution, comprising the following raw materials in parts by weight:
[0036] 8 parts of fatty alcohol polyoxyethylene ether, 1 part of sodium silicate, 0.5 parts of polydimethylsiloxane, 1 part of disodium ethylenediaminetetraacetate, 3 parts of modified silicon dioxide, 65 parts of water;
[0037] The preparation steps are as follows:
[0038] Weigh fatty alcohol polyoxyethylene ether, sodium silicate, polydimethylsiloxane, disodium ethylenediaminetetraacetate, modified silicon dioxide and water in parts by weight and mix them to obtain the product.
[0039] Wherein, the modified silicon dioxide is prepared by the following steps:
[0040] 0.35 g of silica was added to 25 mL of deionized water, and after ultrasonic dispersion and stirring, 1 g of sodium alginate was added, and the mixture was stirred for reaction. After freeze-drying, the mixture was immersed in 40 mL of calcium chloride solution (5 wt %), and the mixture was stirred for reaction for 4 h. The mixture was washed 3 times with deionized water, and dried at 55° C. to obtain modified silica.
[0041] Example 2
[0042] The only difference from Example 1 is that:
[0043] Wherein, the modified silicon dioxide is prepared by the following steps:
[0044] 0.45 g of silica was added to 25 mL of deionized water, and after ultrasonic dispersion and stirring, 1 g of sodium alginate was added, and the mixture was stirred for reaction. After freeze-drying, the mixture was immersed in 40 mL of calcium chloride solution (5 wt %), and the mixture was stirred for reaction for 5 h. The mixture was washed 3 times with deionized water, and dried at 55° C. to obtain modified silica.
[0045] Example 3
[0046] The only difference from Example 1 is that:
[0047] A cleaning solution comprising the following raw materials in parts by weight:
[0048] 12 parts of nonylphenol polyoxyethylene ether, 3 parts of sodium silicate, 0.8 parts of polydimethylsiloxane, 1.5 parts of disodium ethylenediaminetetraacetate, 6 parts of modified silicon dioxide, and 75 parts of water;
[0049] The preparation steps are as follows:
[0050] Weigh nonylphenol polyoxyethylene ether, sodium silicate, polydimethylsiloxane, disodium ethylenediaminetetraacetate, modified silicon dioxide and water in parts by weight and mix them to obtain the product.
[0051] Comparative Example 1
[0052] This comparative example provides a cleaning solution, comprising the following raw materials in parts by weight:
[0053] 8 parts of fatty alcohol polyoxyethylene ether, 1 part of sodium silicate, 0.5 parts of polydimethylsiloxane, 1 part of disodium ethylenediaminetetraacetate, 65 parts of water;
[0054] The preparation steps are as follows:
[0055] Weigh fatty alcohol polyoxyethylene ether, sodium silicate, polydimethylsiloxane, disodium ethylenediaminetetraacetate and water in parts by weight and mix them to obtain the product.
[0056] Comparative Example 2
[0057] The only difference from Example 1 is that:
[0058] A cleaning solution comprising the following raw materials in parts by weight:
[0059] 6 parts of nonylphenol polyoxyethylene ether, 3 parts of sodium silicate, 0.4 parts of polydimethylsiloxane, 1.5 parts of disodium ethylenediaminetetraacetate, 1 part of modified silicon dioxide, and 75 parts of water;
[0060] The preparation steps are as follows:
[0061] Weigh nonylphenol polyoxyethylene ether, sodium silicate, polydimethylsiloxane, disodium ethylenediaminetetraacetate, modified silicon dioxide and water in parts by weight and mix them to obtain the product.
[0062] Example 4
[0063] This embodiment provides a method for increasing the thickness of a heat-treated QPQ compound layer, comprising the following steps:
[0064] The workpiece used in this embodiment is a 30CrMnSiA angle piece.
[0065] S1. Pretreatment: Mechanically remove oil, rust, dry and shot peen the workpiece;
[0066] S2, pre-cleaning: put the workpiece into an ultrasonic cleaning machine containing the cleaning solution obtained in Example 1 for cleaning, wherein the temperature in the ultrasonic cleaning machine is 60°C, the cleaning time is 8 minutes, and after cleaning, the workpiece enters the rinsing tank for rinsing, wherein the rinsing method is to pass compressed air, enter the primary rinsing tank for rinsing with clean water for 5 minutes, then enter the secondary rinsing tank for rinsing with clean water for 2 minutes, and blow dry, wherein the ultrasonic cleaning machine replaces the cleaning solution once every 40 furnaces of cleaning;
[0067] S3, preheating: put the workpiece into the preheating furnace for preheating treatment, the preheating temperature is 360℃, and the preheating time is 180min;
[0068] S4, nitriding: the preheated workpiece is placed in a nitriding furnace for nitriding treatment, the nitriding temperature is 490°C, the nitriding time is 480 min, wherein the nitriding salt is a cyanate-type base salt, and the cyanate concentration is 33%;
[0069] S5, oxidation: After the nitrided workpiece is subjected to salt dripping treatment, it is placed in an oxidation furnace for oxidation treatment at an oxidation temperature of 400°C and an oxidation time of 15 minutes;
[0070] S6, post-cleaning: After the oxidized workpiece is subjected to salt dripping treatment, it is placed in a quenching water tank for quenching cooling, and rinsed after complete cooling. The rinsing method is to pass compressed air into the first rinsing tank for 10 minutes of clean water rinsing, and then into the second rinsing tank for 10 minutes of clean water rinsing, and blow dry. The quenching water tank is changed once every 20 furnaces, the first rinsing tank is changed once every 60 furnaces, and the second rinsing tank is changed once every 80 furnaces;
[0071] S7, closing: closing the workpiece;
[0072] S8, inspection and packaging: Inspect the workpieces, and the processing is completed after passing the quality inspection.
[0073] Example 5
[0074] The only difference from Example 4 is that:
[0075] The cleaning solution in Example 1 in S2 is replaced by the cleaning solution in Example 2.
[0076] Example 6
[0077] The only difference from Example 4 is that:
[0078] The cleaning solution in Example 1 in S2 is replaced by the cleaning solution in Example 3.
[0079] Example 7
[0080] The only difference from Example 4 is that:
[0081] S2. Pre-cleaning: The workpiece is placed in an ultrasonic cleaning machine containing the cleaning solution obtained in Example 1 for cleaning, wherein the temperature in the ultrasonic cleaning machine is 70° C., the cleaning time is 10 min, and the workpiece is placed in a rinsing tank for rinsing after cleaning, wherein the rinsing method is to introduce compressed air, enter the primary rinsing tank for rinsing with clean water for 8 min, then enter the secondary rinsing tank for rinsing with clean water for 3 min, and blow dry, wherein the ultrasonic cleaning machine replaces the cleaning solution once every 40 furnaces of cleaning.
[0082] Example 8
[0083] The only difference from Example 4 is that:
[0084] S3. Preheating: Place the workpiece in a preheating furnace for preheating treatment. The preheating temperature is 370°C and the preheating time is 190 minutes.
[0085] Example 9
[0086] The only difference from Example 4 is that:
[0087] S4. Nitriding: The preheated workpiece is placed in a nitriding furnace for nitriding treatment. The nitriding temperature is 500° C. and the nitriding time is 500 min. The nitriding salt is a cyanate-based salt with a cyanate concentration of 38%.
[0088] Example 10
[0089] The only difference from Example 4 is that:
[0090] S5. Oxidation: After the nitrided workpiece is subjected to salt dripping treatment, it is placed in an oxidation furnace for oxidation treatment. The oxidation temperature is 410°C and the oxidation time is 18 minutes.
[0091] Embodiment 11
[0092] The only difference from Example 4 is that:
[0093] S6. Post-cleaning: After the oxidized workpiece is treated with salt dripping, it is placed in a quenching water tank for quenching and cooling. After complete cooling, it is rinsed by introducing compressed air, entering the first rinsing tank for rinsing with clean water for 15 minutes, and then entering the second rinsing tank for rinsing with clean water for 15 minutes, and then blown dry. The quenching water tank is changed once every 20 furnaces, the first rinsing tank is changed once every 60 furnaces, and the second rinsing tank is changed once every 80 furnaces.
[0094] Comparative Example 3
[0095] The only difference from Example 4 is that:
[0096] The cleaning solution in Example 1 in S2 is replaced by the cleaning solution in Comparative Example 1.
[0097] Comparative Example 4
[0098] The only difference from Example 4 is that:
[0099] The cleaning solution in Example 1 in S2 is replaced by the cleaning solution in Comparative Example 2.
[0100] Comparative Example 5
[0101] The only difference from Example 4 is that:
[0102] S2. Pre-cleaning: The workpiece is placed in an ultrasonic cleaning machine containing the cleaning solution obtained in Example 1 for cleaning, wherein the temperature in the ultrasonic cleaning machine is 50° C., the cleaning time is 15 min, and the workpiece is placed in a rinsing tank for rinsing after cleaning, wherein the rinsing method is to introduce compressed air, enter the primary rinsing tank for rinsing with clean water for 3 min, then enter the secondary rinsing tank for rinsing with clean water for 1 min, and blow dry, wherein the ultrasonic cleaning machine replaces the cleaning solution once every 40 furnaces of cleaning.
[0103] Comparative Example 6
[0104] The only difference from Example 4 is that:
[0105] S3. Preheating: Place the workpiece in a preheating furnace for preheating treatment. The preheating temperature is 330°C and the preheating time is 160 minutes.
[0106] Comparative Example 7
[0107] The only difference from Example 4 is that:
[0108] S4. Nitriding: The preheated workpiece is placed in a nitriding furnace for nitriding treatment. The nitriding temperature is 460° C. and the nitriding time is 520 min. The nitriding salt is a cyanate-based salt with a cyanate concentration of 28%.
[0109] Comparative Example 8
[0110] The only difference from Example 4 is that:
[0111] S5. Oxidation: After the nitrided workpiece is subjected to salt dripping treatment, it is placed in an oxidation furnace for oxidation treatment. The oxidation temperature is 450°C and the oxidation time is 35 minutes.
[0112] Comparative Example 9
[0113] The only difference from Example 4 is that:
[0114] S6. Post-cleaning: After the oxidized workpiece is treated with salt dripping, it is placed in a quenching water tank for quenching and cooling. After complete cooling, it is rinsed by introducing compressed air, entering the first rinsing tank for 5 minutes of clean water rinsing, and then entering the second rinsing tank for 8 minutes of clean water rinsing, and blow-drying. The quenching water tank is changed once every 20 furnaces, the first rinsing tank is changed once every 60 furnaces, and the second rinsing tank is changed once every 80 furnaces.
[0115] The following tests were performed on the workpieces cleaned in step S3 in Examples 4-11 and Comparative Examples 3-9: oil removal rate and corrosion test. The oil removal rate and corrosion test were performed on the obtained workpieces according to the standard JB / T 4323.2-1999. The test results are shown in Table 1:
[0116] Table 1
[0117] project Oil removal rate (%) Corrosiveness / Grade Example 4 98.8 0 Example 5 99.2 0 Example 6 98.6 0 Example 7 98.9 0 Example 8 99.1 0 Example 9 99.3 0 Example 10 99.2 0 Embodiment 11 98.9 0 Comparative Example 3 92.3 0 Comparative Example 4 96.5 0 Comparative Example 5 98.8 0 Comparative Example 6 98.6 0 Comparative Example 7 98.8 0 Comparative Example 8 99.1 0 Comparative Example 9 98.9 0
[0118] The following performance tests were performed on the workpieces obtained in Examples 4-11 and Comparative Examples 3-9: the hardness was measured using a microhardness tester; the wear loss in 1h was measured using a ring-block wear tester; the corrosion current density was measured using the Tafel extrapolation method. The test results are shown in Table 2:
[0119] Table 2
[0120]
[0121]
[0122] It can be seen from the data in Table 1 that the oil removal rate of the workpiece in Comparative Examples 3-4 is lower than that in Examples 4-11. It can be seen that the composition and dosage ratio of the cleaning liquid will affect the cleaning effect of the workpiece. The cleaning liquid prepared by the present invention has an excellent cleaning effect, and its oil removal rate can be as high as 99.3%, which can achieve the cleaning of oil and dirt on the surface of the workpiece, which is helpful for the subsequent processing procedures. It can be seen from the data in Table 2 that the workpiece after the heat treatment QPQ process has a certain infiltration layer thickness. Compared with Comparative Examples 3-4, the workpiece obtained in Example 4-11 has a thicker infiltration layer thickness. It can be seen that whether the workpiece is cleaned cleanly and thoroughly affects the subsequent processing procedures, and then affects the thickness of the compound layer obtained on the surface of the workpiece, and then affects the wear resistance, hardness and corrosion resistance of its compound layer. Compared with Comparative Examples 5-9 and Examples 4-11, it can be seen that the differences in steps and parameters in the process will also affect the thickness of the final infiltration layer and the wear resistance, hardness and corrosion resistance of the compound layer.
[0123] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0124] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for increasing the thickness of a heat-treated QPQ compound layer, characterized in that: The following steps are involved: S1. Pretreatment: Mechanically remove oil, rust, dry and shot peen the workpiece; S2. Pre-cleaning: Put the workpiece into an ultrasonic cleaning machine containing a cleaning solution for cleaning, and then put it into a rinsing tank for rinsing and drying; the cleaning solution includes the following raw materials in parts by weight: 8-12 parts of nonionic surfactant, 1-3 parts of sodium silicate, 0.5-1 parts of polydimethylsiloxane, 1-3 parts of disodium ethylenediaminetetraacetic acid, 3-6 parts of modified silicon dioxide, 65-80 parts of water; S3, preheating: put the workpiece into the preheating furnace for preheating treatment; S4, nitriding: putting the preheated workpiece into a nitriding furnace for nitriding treatment; S5, oxidation: After the nitrided workpiece is subjected to salt dripping treatment, it is placed in an oxidation furnace for oxidation treatment; S6, post-cleaning: After the oxidized workpiece is subjected to salt dripping treatment, it is placed in a quenching water tank for quenching cooling, and after complete cooling, it is rinsed and blown dry; S7, closing: closing the workpiece; S8, inspection and packaging: Inspect the workpieces, and the processing is completed after passing the quality inspection.
2. A method for increasing the thickness of a heat-treated QPQ compound layer according to claim 1, characterized in that: The nonionic surfactant in S2 is at least one of fatty alcohol polyoxyethylene ether, octylphenol polyoxyethylene ether and nonylphenol polyoxyethylene ether.
3. A method for increasing the thickness of a heat-treated QPQ compound layer according to claim 1, characterized in that: The modified silicon dioxide is prepared by the following steps: Add silicon dioxide into deionized water, disperse and stir with ultrasonic, then add sodium alginate, stir to react, freeze-dry and soak in calcium chloride solution, stir to react, wash and dry to obtain modified silicon dioxide.
4. A method for increasing the thickness of a heat-treated QPQ compound layer according to claim 1, characterized in that: The dosage ratio of silicon dioxide, deionized water, sodium alginate and calcium chloride solution is 0.3-0.5 g: 25 mL: 1 g: 40 mL.
5. A method for increasing the thickness of a heat-treated QPQ compound layer according to claim 1, characterized in that: The temperature in the ultrasonic cleaning machine in S2 is 60-70°C and the cleaning time is 8-10 minutes.
6. A method for increasing the thickness of a heat-treated QPQ compound layer according to claim 1, characterized in that: The S2 rinsing method is: introduce compressed air, enter the primary rinsing tank for rinsing with clean water for 5-8 minutes, and then enter the secondary rinsing tank for rinsing with clean water for 2-3 minutes.
7. A method for increasing the thickness of a heat-treated QPQ compound layer according to claim 1, characterized in that: The preheating temperature in S3 is 360±10℃, and the preheating time is 180-200min.
8. A method for increasing the thickness of a heat-treated QPQ compound layer according to claim 1, characterized in that: In S4, the nitriding temperature is 490±10℃ and the nitriding time is 480-500min; The S4 nitriding furnace uses a nitriding salt for nitriding reaction, wherein the nitriding salt is a cyanate-type base salt, wherein the cyanate concentration is 32%-39%.
9. A method for increasing the thickness of a heat-treated QPQ compound layer according to claim 1, characterized in that: The oxidation temperature in S5 is 400±10°C and the oxidation time is 15-20min.
10. A method for increasing the thickness of a heat-treated QPQ compound layer according to claim 1, characterized in that: The specific method of rinsing in S6 is: introducing compressed air, entering the first rinsing tank for rinsing with clean water for 10-15 minutes, and then entering the second rinsing tank for rinsing with clean water for 1-5 minutes.