One-time forming current collector composite film preparation device and coating method
By designing a single-formed current collector composite film preparation device, double-sided disposable coating of the substrate is achieved by using dense boat arrangement and multi-evaporation device, the problems of poor plating density and low production efficiency in the prior art are solved, and composite aluminum foil is improved physical performance and production efficiency.
Patent Information
- Application Number
- CN202410908945.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-22
AI Technical Summary
The existing composite aluminum foil production process cannot achieve double-sided single-use coating of the substrate, and there are problems such as poor plating density, reduced physical performance, low production efficiency, and high cost.
A single-formed current collector composite film preparation device is designed, including a winding chamber, a vacuum chamber, an evaporation chamber and a controller. The number of evaporation boats is increased through the arrangement of dense boats, multiple evaporation devices and coating drums are set up, and thickness measuring instruments are used. The temperature measurement device monitors and close-loop controls the temperature of the wire feeding device and the evaporation boat in real time to realize double-sided disposable coating of the substrate.
The double-sided disposable coating of the substrate is realized, which improves the density and physical properties of the coating, simplifies production steps, improves production efficiency and reduces costs.
Smart Images

Figure CN118996337A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of current collectors, and in particular to a one-step forming current collector composite film preparation device and a coating method. Background Art
[0002] Composite aluminum foil generally adopts the roll-to-roll vacuum evaporation coating process, with high-purity aluminum wire as the evaporation material and evaporation boat as the evaporation source. Aluminum is deposited on the surface of flexible substrates such as PET, PP, PE, PI, etc. in the vacuum evaporation chamber of the evaporation equipment by evaporation under high vacuum. The thickness of the metal aluminum layer deposition has different requirements according to different application fields. Especially in the field of lithium batteries, composite aluminum foil is a new key current collector material for the production of lithium batteries, and the aluminum coating layer on both sides of the PET film is required to reach a thickness of 1μm. The production and molding process of composite aluminum foil currently used for lithium battery current collector materials mostly adopts multiple single-sided vacuum suspension evaporation coating and vacuum drum evaporation coating methods, that is, a roll of PET base film is evaporated from beginning to end under vacuum environment. After the aluminum coating is completed, the evaporation equipment is broken, and then the film with a layer of aluminum metal evaporated on the winding end is placed back to the unwinding section of the equipment, and the previous coating process is repeated to achieve a final coating thickness of 1μm.
[0003] In the vacuum suspension evaporation method, the single coating thickness is 40 to 70nm, and it takes 30 to 38 cycles of evaporation to achieve the 1000nm coating thickness requirement. Multiple evaporation passes can easily cause accumulation of spatter holes on the surface of the film material. At the same time, during the multiple coating processes, the polymer material is heated and crystallized multiple times, resulting in a decrease in physical properties such as elongation and tensile strength. In addition, the cycle is long, the process is complicated, and it is not suitable for large-scale mass production.
[0004] The defects of the vacuum drum plating method are that the drum is not firmly attached and it is easy to produce empty plating lines and wrinkles. In addition, the single-row evaporation source and single-row wire feeding device distribution structure and the width of the wire feeding device cause the evaporation source arrangement distance to be large and the evaporation points to be few, resulting in a single deposition thickness of ≤200nm, low vapor saturation pressure of the coating material, and poor density of the coating.
[0005] In the above two traditional processes, the substrate surface needs to be corona pre-treated and oxidized before plating to increase the surface tension. The process is cumbersome and complicated, with a low degree of intelligence and a large influence of human factors. In addition, both processes have the disadvantages of low production efficiency, high cost, and the film material is easily contaminated or damaged during the inversion process.
[0006] Based on the above considerations, it is urgent to develop an efficient, automated, intelligent, digital, one-time forming process and device for preparing micron-level layer-thick composite aluminum foil to increase production and efficiency to meet the needs of industry development. Summary of the invention
[0007] The technical problem to be solved by the present invention is to solve the problem that the existing process cannot realize one-time coating on both sides of the substrate.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0009] A one-step forming current collector composite film preparation device comprises a winding chamber (1200), a vacuum chamber (300), an evaporation chamber (400), a track (500) and a controller; the vacuum chamber (300) is located between the winding chamber (1200) and the evaporation chamber (400); and when working, the winding chamber (1200) and the evaporation chamber (400) enter the vacuum chamber (300) along the track (500) to perform a coating operation;
[0010] Wherein, the winding chamber (1200) is provided with an unwinding roller (110), a plurality of first side coating drums (120), a first side thickness measuring piece (130), a plurality of second side coating drums (210), a second side thickness measuring piece (220) and a winding roller (230) in sequence according to the process flow; and includes a plurality of flattening rollers (140) distributed between the devices in the winding chamber (1200);
[0011] The evaporation chamber (400) comprises a first evaporation chamber (410) and a second evaporation chamber (420), a telescopic partition (430) being arranged between the two evaporation chambers; and each evaporation chamber is provided with a plurality of evaporation devices (440), a plurality of wire feeding devices (450) and a plurality of temperature measuring devices (460);
[0012] and the evaporation surfaces of the plurality of evaporation devices (440) in the first evaporation chamber (410) face the bottoms of the plurality of first side coating drums (120), and the evaporation surfaces of the plurality of evaporation devices (440) in the second evaporation chamber (420) face the bottoms of the plurality of second side coating drums (210);
[0013] The controller is communicatively connected with the first side thickness measuring piece (130), the second side thickness measuring piece (220), a plurality of evaporating devices (440), a plurality of wire feeding devices (450), and a plurality of temperature measuring devices (460).
[0014] Advantages: By arranging the evaporation boats closely together, the number of evaporation boats can be increased, the heat energy can be evenly shared, and the physical properties of the film can be improved. The number of evaporation devices and coating drums can be increased, and the thickness of the deposited coating can be accumulated. During the process, the thickness gauge and temperature measuring device can be used for real-time monitoring, and the controller can control the conveying rate of the wire feeding device and the temperature of the evaporation boat in a closed loop to ensure the uniformity of the coating.
[0015] During the winding production, the transmission device is used to turn the film material over during the process to complete the evaporation on both sides, avoiding transportation wear and contamination, streamlining the process, and in the process, the thickness gauge and PLC intelligent closed-loop control the thickness and uniformity of the deposition layer, and the temperature meter and PLC intelligent closed-loop control the evaporation temperature to ensure the optimal performance of the composite aluminum foil.
[0016] In one embodiment of the present invention, at least two first side coating drums (120) are arranged side by side, and a biasing device is provided in the first side coating drum (120); at least two second side coating drums (210) are arranged side by side, and a biasing device is provided in the second side coating drum (210); and an evaporation device (440) is provided at the bottom of each first side coating drum (120) and each second side coating drum (210).
[0017] In one embodiment of the present invention, a first lithium ion processor (150) is arranged between the unwinding roller (110) and the first side coating drum (120); a second lithium ion processor (240) is arranged between the first side thickness measuring piece (130) and the second side coating drum (210), and the first lithium ion processor (150) and the second lithium ion processor (240) respectively remove dust and static electricity from different sides of the base film (600).
[0018] In one embodiment of the present invention, a first low vacuum chamber (160) and a second low vacuum chamber (250) are arranged in the winding chamber (1200); wherein the first low vacuum chamber (160) is located between the first side coating drum (120) and the first side thickness measuring piece (130); the second low vacuum chamber (250) is located between the second side coating drum (210) and the second side thickness measuring piece (220); and a first auxiliary cooling roller (161) is arranged in the first low vacuum chamber (160), and a second auxiliary cooling roller (251) is arranged in the second low vacuum chamber (250).
[0019] In one embodiment of the present invention, each evaporation device (440) includes an evaporation tank (441), a plurality of evaporation seats (442) are arranged in the evaporation tank (441), an evaporation boat (443) is clamped on the evaporation seat (442), and the step of the evaporation seat (442) is parallel to the evaporation boat (443), and the plurality of evaporation boats (443) are evenly arranged corresponding to the lateral width of the base film (600).
[0020] In one embodiment of the present invention, a baffle plate (1210) is provided in the winding chamber (1200), and the baffle plate (1210) is located below a plurality of first side coating drums (120) and a plurality of second side coating drums (210), and a plurality of coating drum grooves (1210) are provided on the baffle plate (1210), and the bottoms of the plurality of first side coating drums (120) are exposed to the first evaporation chamber (410) through the plurality of coating drum grooves (1210), and the bottoms of the plurality of second side coating drums (210) are exposed to the second evaporation chamber (420) through the plurality of coating drum grooves (1210).
[0021] In one embodiment of the present invention, a plurality of evaporation baffles (1220) located below the baffle plate (1210) are disposed in the winding chamber (1200), and an evaporation baffle (1220) is disposed on each evaporation device (440).
[0022] In one embodiment of the present invention, the evaporation seat (442) has a width of 35-40 mm, a length of 30-50 mm, and a height of 30-50 mm; the evaporation boat (443) has a width of 35-40 mm, a length of 130-150 mm, and a center distance between two adjacent evaporation boats (443) of 40-50 mm.
[0023] In one embodiment of the present invention, a plurality of wire feeding devices (450) are arranged on both sides of the evaporation tank (441), each evaporation boat (443) is equipped with a wire feeding device (450), and the wire feeding devices (450) are arranged in a staggered manner on the evaporation tank (441).
[0024] The present invention also provides a coating method for a one-step forming current collector composite film preparation device, comprising:
[0025] After placing the base film (600) on the unwinding roller (110), close the vacuum chamber (300), open the telescopic partition (430), and start vacuuming; simultaneously start the biasing devices in the multiple first side coating drums (120) and the multiple second side coating drums (210), then start the multiple evaporation devices (440) and the multiple wire feeding devices (450) in the first evaporation chamber (410) and the second evaporation chamber (420), start the winding roller (230), and the multiple flattening rollers (140) to transfer the base film (600); after the evaporation device (440) reaches a suitable temperature, perform evaporation;
[0026] During the evaporation process, the controller obtains data fed back by a plurality of temperature measuring devices (460), a first side thickness measuring piece (130), and a second side thickness measuring piece (220), compares the data with a set evaporation temperature range and a preset film thickness, and adjusts the power output of the evaporation device (440) and the wire feeding speed of the wire feeding device (450) according to the comparison result.
[0027] Compared with the prior art, the beneficial effects of the present invention are as follows: during the coating process of the base film of the present invention, the process flow includes "entering the warehouse - plasma treatment (increasing surface tension and removing dust and static electricity) - coating and cooling of the first side of the multi-evaporation device - information feedback and automatic adjustment - plasma treatment (dust removal and static electricity removal) - coating and cooling of the second side of the multi-evaporation device - information feedback and automatic adjustment - exiting the warehouse". The whole process flow is used to achieve one-time coating of both sides of the substrate, and the number of evaporation boats is increased by arranging the boats closely, the heat energy is evenly shared, the physical properties of the film are improved, the number of evaporation devices and coating drums is increased, and the thickness of the deposited coating is accumulated. During the process, the thickness meter and the temperature measuring device are monitored in real time, and the controller controls the conveying rate of the wire feeding device and the temperature of the evaporation boat in a closed loop to ensure the uniformity of the coating. At the same time, the setting of the low vacuum chamber and the auxiliary cooling roller strengthens and accelerates the solidification and deposition of the attached metal particles, thereby achieving efficient one-time evaporation processing to reach full production and efficiency.
[0028] In the winding production process, the transmission device is used to turn the film material over to complete the evaporation on both sides, avoiding transportation wear and contamination, streamlining the process, and in the process, the thickness gauge and PLC system closed-loop control the thickness and uniformity of the deposition layer, and the temperature measuring device and PLC system closed-loop control the evaporation temperature to ensure the optimal performance of the composite film.
[0029] Achieve 1μm evaporation molding in one time, simplify production steps and improve production efficiency. It is equipped with independent evaporation chamber, winding chamber and low vacuum chamber. By controlling the telescopic partition, two independent evaporation chambers are formed after closing the chamber, which isolates the metal atoms and escaped molecules in the front and back coating areas, stabilizes the vacuum flocculent flow, and reduces the escape rate. The film surface after coating enters an independent low vacuum chamber. Under the dual effects of pressure and auxiliary cooling roller, it is secondary condensed to strengthen and accelerate the condensation of metal particles, making the adhesion firmer. Dense boat evaporation reduces the evaporation temperature, so that the heat energy is evenly shared and the physical properties of the composite film are improved. The evaporation device, wire feeding device and coating drum are a set of evaporation systems, which can be set from 2 groups, 4 groups, 6 groups, 8 groups... to N groups, and the evaporation rate multiplier increases. It can be used alone or in multiple combinations. It can be single-sided coating, double-sided coating at the same time, double-sided coating thickness differentiation coating, or two-sided coating with different coating materials or multi-material mixed coating. The multi-evaporation system can easily realize one-time forming processing of different coating thicknesses, such as composite aluminum film, composite copper film, and other composite films with different coating thickness requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Schematic diagram of a one-step forming current collector composite membrane preparation device according to an embodiment of the present invention.
[0031] Figure 2 Schematic diagram of a winding chamber according to an embodiment of the present invention.
[0032] Figure 3 It is a schematic diagram of an evaporation device and a wire feeding device according to an embodiment of the present invention.
[0033] Figure 4 Schematic diagram of an evaporation boat and an evaporation seat according to an embodiment of the present invention. DETAILED DESCRIPTION
[0034] In order to facilitate those skilled in the art to understand the technical solution of the present invention, the technical solution of the present invention is further described in conjunction with the accompanying drawings of the specification.
[0035] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0036] Example 1
[0037] See also Figure 1 and Figure 2 As shown, the present invention provides a one-step forming current collector composite film preparation device, comprising a winding chamber 1200, a vacuum chamber 300, an evaporation chamber 400, a track 500 and a controller. The vacuum chamber 300 is located between the winding chamber 1200 and the evaporation chamber 400, and when working, the winding chamber 1200 and the evaporation chamber 400 enter the vacuum chamber 300 along the track 500 to perform the coating operation.
[0038] Among them, the winding chamber 1200 is provided with an unwinding roller 110, multiple first side coating drums 120, a first side thickness measuring piece 130, multiple second side coating drums 210, a second side thickness measuring piece 220 and a winding roller 230 in sequence according to the process flow, as well as multiple flattening rollers 140, which are distributed between the various devices in the winding chamber 1200.
[0039] The evaporation chamber 400 includes a first evaporation chamber 410 and a second evaporation chamber 420, a telescopic partition 430 is arranged between the two evaporation chambers, and each evaporation chamber is provided with a plurality of evaporation devices 440, a plurality of wire feeding devices 450 and a plurality of temperature measuring devices 460. When the telescopic partition 430 is in operation, it is in an expanded state, which plays a role in isolating the first evaporation chamber 410 and the second evaporation chamber 420, preventing the metal particles between the first evaporation chamber 410 and the second evaporation chamber 420 from escaping from each other and generating floccules, and preventing the pressure difference between the first evaporation chamber 410 and the second evaporation chamber 420 from generating convection, which affects the stability of evaporation.
[0040] And the evaporation surfaces of the multiple evaporation devices 440 in the first evaporation chamber 410 face the bottoms of the multiple first side coating drums 120, and the evaporation surfaces of the multiple evaporation devices 440 in the second evaporation chamber 420 face the bottoms of the multiple second side coating drums 210. Specifically, the multiple evaporation devices 440 all play the role of evaporating metal particles, and the evaporation devices 440 can be set in n groups where n is a multiple of 2. In theory, the more the number of evaporation devices 440, the greater the evaporation amount, the better the coating effect, and the thicker the one-time deposition layer. The sum of the number of the multiple first side coating drums 120 and the multiple second side coating drums 210 corresponds to the number of the multiple evaporation devices 440, that is, each first side coating drum 120 corresponds to an evaporation device 440, and each second side coating drum 210 also corresponds to an evaporation device 440.
[0041] The controller is in communication connection with the first side thickness measuring member 130, the second side thickness measuring member 220, a plurality of evaporation devices 440, a plurality of wire feeding devices 450 and a plurality of temperature measuring devices 460. Specifically, the controller is a PLC device.
[0042] See also Figures 1 to 4 As shown, in one embodiment of the present invention, a first lithium ion processor 150 is arranged between the unwinding roller 110 and the first side coating drum 120, and a second lithium ion processor 240 is arranged between the first side thickness measuring piece 130 and the second side coating drum 210, and the first lithium ion processor 150 and the second lithium ion processor 240 respectively remove dust and static electricity from different sides of the base film 600.
[0043] The winding chamber 1200 is provided with a first low vacuum chamber 160 and a second low vacuum chamber 250, wherein the first low vacuum chamber 160 is located between the first side coating drum 120 and the first side thickness measuring piece 130, and the second low vacuum chamber 250 is located between the second side coating drum 210 and the second side thickness measuring piece 220. In addition, a first auxiliary cooling roller 161 is provided in the first low vacuum chamber 160, and a second auxiliary cooling roller 251 is provided in the second low vacuum chamber 250.
[0044] A cryogenic device, a refrigeration system and a vacuum system are also provided in the vacuum chamber 300. A cryogenic device is provided in both the first evaporation chamber 410 and the second evaporation chamber 420 to capture water, oil vapor and dust, accelerate conversion and purify vacuum, and the vacuum system is used to evacuate the vacuum chamber 300. A transmission device 170 is provided in the winding chamber 1200 to transmit the base film 600.
[0045] The first low vacuum chamber 160 and the second low vacuum chamber 250 are both connected to the vacuum system to change the internal pressure of the vacuum chamber 300. The first auxiliary cooling roller 161 and the second auxiliary cooling roller 251 are both connected to the refrigeration system to cool the film material and accelerate the deposition of metal particles.
[0046] In this embodiment, a baffle plate 1210 is provided in the winding chamber 1200, and the baffle plate 1210 is located below the multiple first side coating drums 120 and the multiple second side coating drums 210, and a multiple coating drum grooves 1210 are provided on the baffle plate 1210, and the bottoms of the multiple first side coating drums 120 are exposed to the first evaporation chamber 410 through the multiple coating drum grooves 1210, and the bottoms of the multiple second side coating drums 210 are exposed to the second evaporation chamber 420 through the multiple coating drum grooves 1210.
[0047] The winding chamber 1200 is provided with a plurality of evaporation baffles 1220 located below the blocking plate 1210, and each evaporation device 440 is provided with an evaporation baffle 1220. The evaporation baffle 1220 protects the base film 600 at the beginning and end of evaporation to prevent the base film 600 from being damaged by high temperature.
[0048] In this embodiment, at least two first side coating drums 120 are arranged side by side, and bias devices are arranged in the first side coating drums 120, at least two second side coating drums 210 are arranged side by side, and bias devices are arranged in the second side coating drums 210, and an evaporation device 440 is arranged at the bottom of each first side coating drum 120 and each second side coating drum 210. In this embodiment, two first side coating drums 120 and two second side coating drums 210 are arranged, so there is no doubt that four evaporation devices 440 are arranged.
[0049] In this embodiment, each evaporation device 440 includes an evaporation tank 441, and a plurality of evaporation seats 442 are arranged in the evaporation tank 441. An evaporation boat 443 is clamped on the evaporation seat 442, and the step of the evaporation seat 442 is parallel to the evaporation boat 443, and the plurality of evaporation boats 443 are evenly arranged corresponding to the lateral width of the base film 600. A pair of evaporation seats 442 clamps one evaporation boat 443. The evaporation seats 442 are made of highly conductive copper and are connected to a cooling device to maintain the resistivity of the evaporation seat 442 under control.
[0050] A plurality of wire feeding devices 450 are arranged on both sides of the evaporation tank 441. Each evaporation boat 443 is equipped with a wire feeding device 450, and they are staggered on the evaporation tank 441 to shorten the spacing. The wire feeding direction is consistent with the length direction of the evaporation boat 443, minimizing the impact of the forward and backward movement of the aluminum wire on evaporation.
[0051] The evaporation seat 442 has a width of 35-40 mm, a length of 30-50 mm, and a height of 30-50 mm; the evaporation boat 443 has a width of 35-40 mm, a length of 130-150 mm, and a height of 10 mm, and the center distance between two adjacent evaporation boats 443 is 40-50 mm.
[0052] When the lateral width of the base film 600 is 1200-1800 mm, the evaporation boat 443 with a width of 35-40 mm is selected, and the number of the evaporation boats 443 is 27-36.
[0053] The coating thickness rule is: when coating the base film 600, if the coating is relatively thick, a 40mm×150mm wide and long evaporation boat 443 is selected; if the coating is relatively thin, a 35mm×130mm wide and long evaporation boat 443 is used; and in both cases, the interval between the sides of two adjacent evaporation boats 443 is ≥10mm, and the lateral interval of the evaporation seat 442 is ≥5mm.
[0054] By setting up multiple evaporation devices 440 and closely arranging evaporation boats 443 on each of the multiple evaporation devices 440, one-time coating forming is achieved. The working principle of the closely arranged boats is: under the same vacuum (pressure) and the same wire feeding amount (liquid volume), the area is proportional to the evaporation rate, and under the same vacuum (pressure) and the same evaporation boat (area), the volume (liquid height) is inversely proportional to the evaporation rate. In addition, under the same vacuum and temperature, the evaporation rate (limit) of the substance is certain, so increasing the wire feeding amount (volume) requires increasing the area of the evaporation boat. The volume (liquid height) is inversely proportional to the evaporation rate, that is, the shallower the depth, the higher the evaporation rate. In addition, the liquid spreading area is proportional to the height, which affects the evaporation rate. The liquid cannot be high, so the spreading area is limited, so the evaporation boat area can only be maintained within a certain range.
[0055] Under a certain vacuum, the higher the temperature, the faster the evaporation rate, which is achieved by increasing the temperature of the evaporation boat, Q = cm△t, where Q is heat, c is specific heat capacity, m is the mass of the object, and △t is the temperature change of the object. The specific heat capacity c and mass m remain unchanged. The higher the temperature, the greater the heat absorbed by the film deposition, resulting in deformation and decreased physical properties. Molecular distillation focuses on evaporation in the vertical direction, and the base film absorbs more heat in the area perpendicular to the evaporation boat. Based on the law of conservation of energy, the heat energy brought by the increase in the evaporation boat does not disappear, but is shared more evenly. By lowering the temperature and reducing the evaporation rate, the Q value decreases by the same △t ratio, reducing the heat energy absorbed by the film material perpendicular to the evaporation boat. Therefore, the multi-evaporation boat method allows the base film 600 to share the heat energy evenly, which can improve the physical properties of the product; multiple evaporation devices accumulate the deposition thickness, and multiple evaporation devices are arranged in dense boats to achieve a double increase in efficiency and performance.
[0056] In this embodiment, the temperature measuring device 460 may be a temperature sensor or an infrared thermometer, which is connected to the controller to achieve temperature control of the evaporation boat 443 .
[0057] When the temperature measuring device 460 is a temperature sensor, during the evaporation process, an electric potential is generated by the temperature sensor close to the bottom of each evaporation boat 443, and the electric signal is amplified by the internal OP amplifier and converted into a temperature value by the electrical instrument (secondary instrument). At the same time, the signal is fed back to the controller, and the controller is written with the evaporation temperature range set by the program: evaporation vacuum value: 5.0×10 -4 --1.0×10 -2 The corresponding evaporation temperature range is 812-972° C. The controller is a three-phase power regulator of the evaporation boat 443, which adjusts the power output to achieve closed-loop control of the evaporation temperature.
[0058] When the temperature measuring device 460 is an infrared thermometer, the temperature of the evaporation boat 443 is displayed by the installed infrared thermometer, and the signal is fed back to the controller. The evaporation temperature range set by the program written into the controller is: evaporation vacuum value: 5.0×10 -4 -1.0×10 -2 The corresponding evaporation temperature range is 812-972°C. The three-phase power regulator of the controller evaporation boat 443 adjusts the power output to achieve closed-loop control of the evaporation temperature. The advantage is that the infrared thermometer responds quickly and the temperature controller is convenient for temperature setting and modification.
[0059] In this embodiment, the first side thickness measuring piece 130 and the second side thickness measuring piece 220 are both intelligent thickness gauges, which collect data and output them in the form of electrical signals, which are sent to the display and the automatic thickness control system through the matrix switcher VGA. The display shows the film thickness square resistance value of each evaporation boat 443 corresponding to the area, and the automatic thickness control controls the wire feeding speed of each wire feeding motor in the multiple wire feeding devices 450 through the incremental controller in a closed loop to increase or decrease the evaporation amount until the film thickness measured by the first side thickness measuring piece 130 and the second side thickness measuring piece 220 reaches the preset film thickness, thereby realizing closed-loop automatic control of the coating thickness. In this embodiment, when feeding aluminum wire, the 1μm aluminum layer is 36-37mΩ.
[0060] See also Figures 1 to 4 As shown, the present invention also provides a coating method for a one-time forming current collector composite membrane preparation device, comprising:
[0061] After placing the base film 600 on the unwinding roller 110, close the vacuum chamber 300, open the telescopic partition 430, and start vacuuming; at the same time, start the bias devices in the multiple first side coating drums 120 and the multiple second side coating drums 210, then start the multiple evaporation devices 440 and the multiple wire feeding devices 450 in the first evaporation chamber 410 and the second evaporation chamber 420, start the winding roller 230, and the multiple flattening rollers 140 to transfer the base film 600, and after the evaporation device 440 reaches a suitable temperature, perform vapor deposition.
[0062] During the evaporation process, the controller obtains the data fed back by the multiple temperature measuring devices 460, the first side thickness measuring device 130, and the second side thickness measuring device 220, and compares them with the set evaporation temperature range and the preset film thickness, and adjusts the power output of the evaporation device 440 and the wire feeding speed of the wire feeding device 450 according to the comparison results. Among them, the temperature and wire feeding speed are prohibited from being controlled synchronously, and the temperature control is performed first, and then the wire feeding speed control is performed.
[0063] Specifically, in this embodiment, the winding length is set, which is 1000 meters in this embodiment. After the base film 600 is placed in the unwinding roller 110, the vacuum chamber 300 is closed, the evaporation baffle 1220 is closed, the telescopic partition 430 is opened, the vacuum system is started, and the vacuum chamber 300 is evacuated to 1.0×10 -1 Pa, the first evaporation chamber 410 and the second evaporation chamber 420 are at 7.5×10 -3 Pa, the first low vacuum chamber 160 and the second low vacuum chamber 250 are evacuated to 1-10 Pa. In this embodiment, the first evaporation chamber 410 and the second evaporation chamber 420 are evacuated to 5×10 -3 Pa, the first low vacuum chamber 160 and the second low vacuum chamber 250 are evacuated to 5Pa, and the deep cooling device is turned on at the same time. The voltage of the bias device in the first side coating drum 120 and the second side coating drum 210 is set to 100-500V, 360V in this embodiment. The cooling temperature is -10 to 50°C, 15°C in this embodiment, and it is started.
[0064] The parameters of the multiple first side coating drums 120 and the multiple second side coating drums 210 are set to be the same, with a voltage of 200-400V, a current of 20-40A, a power of 50-80% and a temperature of 8888888°C. In this embodiment, the voltage is 280V, the current is 28A, the power is 70%, the temperature is 970°C, and they are started. After reaching the evaporation temperature, the temperature of the evaporation boat 443 in this embodiment reaches 900°C, and the multiple wire feeding devices 450 are started. The wire feeding speed of the multiple wire feeding devices 450 is 100-500mm / min. In this embodiment, the wire feeding speed is 300mm / min. All rollers from the unwinding roller 110 to the winding roller 230 are turned on for trial winding. Among them, the cooling temperature of the first auxiliary cooling roller 161 is -10-20°C, and the cooling temperature of the second auxiliary cooling roller 251 is 10-25°C. The parameter setting range of the first lithium ion processor 150 and the second lithium ion processor 240 is 200-300V voltage, 1-8A current, 100-1000cc argon flow rate, and 0.1-0.5MPa pressure. In this embodiment, the voltage of the first lithium ion processor 150 is 240V, the current is 5A, the argon flow rate is 400cc, the pressure is 0.4MPa and it is turned on. The voltage of the second lithium ion processor 240 is 220V, the current is 3A, the argon flow rate is 100cc, the pressure is 0.3MPa and it is turned on.
[0065] The test run is normal, the winding is turned on, the winding speed is 27m / min, the baffle plate 1210 is opened, and the base film 600 is at the bottom of the multiple first side coating drums 120, after multiple evaporation, cooling and deposition, and circulates to the first auxiliary cooling roller 161 for reinforcement deposition again. The controller is started for automatic control, and the temperature of the evaporation boat 443 in the first evaporation chamber 410 is controlled by the feedback data of the temperature measuring device 460 in the first evaporation chamber 410. The base film 600 circulates to the first side thickness measuring piece 130 to display the feedback coating thickness, and the controller controls the wire feeding speed of the wire feeding device 450 in the first evaporation chamber 410.
[0066] The base film 600 is turned over and in the winding chamber 1200, it is driven, flattened, and turned over by a plurality of flattening rollers 140 and a transmission device 170, so that the side of the film on which metal particles are not deposited is turned over to the bottom of a plurality of second side coating drums 210, so as to facilitate the subsequent metal particle coating on the other side of the base film 600.
[0067] After the single-sided coating is completed, it passes through the transmission device 170 and multiple flattening rollers 140 and enters the second lithium ion processor 240. After dust removal and static electricity removal, it enters the bottom of multiple second side coating drums 210. After multiple evaporation, cooling and deposition, it enters the second low vacuum chamber 250 and is reinforced and condensed on the second auxiliary cooling roller 251. At this point, the double-sided coating is completed. The controller feeds back data through the temperature measuring device 460 located in the second evaporation chamber 420 to execute the temperature control of the evaporation boat 443 in the second evaporation chamber 420. The coating cycle is fed back to the second side thickness measuring piece 220 to display the feedback coating thickness, and the controller controls the wire feeding speed of the wire feeding device 450 in the second evaporation chamber 420. The base film 600 is automatically wound from unwinding to winding, and the controller automatically closes the loop to adjust the evaporation temperature and thickness.
[0068] The winding stops at 1000m, the evaporation baffle 1220, all wire feeding devices 450 and evaporation boat 443 are automatically closed, the cryogenic device and the refrigeration system are automatically heated up to room temperature, the thickness measuring piece and the lithium ion processor are stopped and the argon gas is turned off, the vacuum is broken and the one-time double-sided vapor deposition molding process is completed, and both sides of the composite film reach the 1μm level in one production process.
[0069] Example 2
[0070] Although Example 1 can achieve the purpose of real-time monitoring of the thickness of the evaporated film, there is a lag. If the base film itself has defects, it can only detect the coating after vapor deposition. Even if there is an area with unqualified layer thickness, it cannot be repaired. It can only ensure that unqualified film thickness will not continue to occur in the future. Therefore, it is necessary to detect whether there are defects on the surface of the base film at the front end of vapor deposition, and thicken the coating at the defective part to avoid defective products.
[0071] See also Figures 1 to 4 As shown, on the basis of Example 1, this Example 2 further includes a data acquisition module and a target detection algorithm model. Among them, the data acquisition module sets the area before the base film 600 is coated, which is used to obtain the surface image of the base film 600 before evaporation in real time as a data set. The target detection algorithm model is applied to the defect detection on the surface of the base film 600, and the target detection algorithm model is connected to the controller through a server interface. If there are defects in the image of the base film 600, the base film 600 is subjected to surface defect detection, and the controller controls the evaporation device 440 to increase the power and increase the thickness of the evaporated coating to avoid the coating thickness caused by the surface defects of the base film 600 being lower than the minimum thickness value of the qualified product standard, thereby achieving the goal of avoiding the defective parts of the entire roll of coating caused by the defects of the base film 600 itself before evaporation.
[0072] Furthermore, the surface defects of the base film 600 include scratches, marks, dirt, and concave / convex spots.
[0073] The target detection algorithm model based on deep learning detects surface defects of the base film 600, including the following steps:
[0074] S1, the data acquisition module collects data: takes photos of the base film with scratches, nicks, dirt, concave / convex spots and qualified base film as a data set, and divides the data set into a training set, a test set and a validation set;
[0075] S2, model selection, using Faster R-CNN as the backbone network model, Resnet152 as the backbone feature extraction network model, using mean average precision mAP as the evaluation index, setting the batch size to 50, the training epoch to 500, and the categories of the data set to 6; obtaining the proposed box network through training with the training set, using ROI to obtain the prediction results, and then retraining the network with the prediction results, detecting the test set photos, generating the detection results of each photo, generating the corresponding prediction box file, and then taking the label file in the test set, generating the text file of the real box according to the result of each label file, calculating the overlap degree of all the proposed boxes and the real boxes, and screening, setting confidence to 0.5, the proposed boxes with an overlap degree greater than 0.5 are qualified basement membrane photos, and the proposed boxes with an overlap degree less than 0.5 are defective basement membrane photos, and finally obtaining the mAP value, and then setting the validation set to verify the trained model to obtain the best target detection algorithm model.
[0076] S3, applying the optimal target detection algorithm model to detect surface defects of the base film, and transmitting the detection results to the controller, which increases the power of the evaporation device 440 in the corresponding area to increase the thickness of the evaporated coating.
[0077] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-limiting from any point of view, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention, and any reference numerals in the claims should not be regarded as limiting the claims involved.
[0078] The above-described embodiments merely represent implementation methods of the invention. The protection scope of the present invention is not limited to the above-described embodiments. For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A one-step forming current collector composite membrane preparation device, characterized in that: The invention comprises a winding chamber (1200), a vacuum chamber (300), an evaporation chamber (400), a track (500) and a controller; the vacuum chamber (300) is located between the winding chamber (1200) and the evaporation chamber (400); and when working, the winding chamber (1200) and the evaporation chamber (400) enter the vacuum chamber (300) along the track (500) to perform a coating operation; Wherein, the winding chamber (1200) is provided with an unwinding roller (110), a plurality of first side coating drums (120), a first side thickness measuring piece (130), a plurality of second side coating drums (210), a second side thickness measuring piece (220) and a winding roller (230) in sequence according to the process flow; and includes a plurality of flattening rollers (140) distributed between the devices in the winding chamber (1200); The evaporation chamber (400) comprises a first evaporation chamber (410) and a second evaporation chamber (420), a telescopic partition (430) being arranged between the two evaporation chambers; and each evaporation chamber is provided with a plurality of evaporation devices (440), a plurality of wire feeding devices (450) and a plurality of temperature measuring devices (460); and the evaporation surfaces of the plurality of evaporation devices (440) in the first evaporation chamber (410) face the bottoms of the plurality of first side coating drums (120), and the evaporation surfaces of the plurality of evaporation devices (440) in the second evaporation chamber (420) face the bottoms of the plurality of second side coating drums (210); The controller is communicatively connected with the first side thickness measuring piece (130), the second side thickness measuring piece (220), a plurality of evaporating devices (440), a plurality of wire feeding devices (450), and a plurality of temperature measuring devices (460).
2. The one-step forming current collector composite membrane preparation device according to claim 1, characterized in that: At least two first side coating drums (120) are arranged side by side, and a biasing device is arranged inside the first side coating drum (120); at least two second side coating drums (210) are arranged side by side, and a biasing device is arranged inside the second side coating drum (210); and an evaporation device (440) is arranged at the bottom of each first side coating drum (120) and each second side coating drum (210).
3. The one-step forming current collector composite membrane preparation device according to claim 1, characterized in that: A first lithium ion processor (150) is arranged between the unwinding roller (110) and the first side coating drum (120); a second lithium ion processor (240) is arranged between the first side thickness measuring piece (130) and the second side coating drum (210), and the first lithium ion processor (150) and the second lithium ion processor (240) respectively remove dust and static electricity from different sides of the base film (600).
4. The one-step forming current collector composite membrane preparation device according to claim 1, characterized in that: A first low vacuum chamber (160) and a second low vacuum chamber (250) are arranged in the winding chamber (1200); wherein the first low vacuum chamber (160) is located between the first side coating drum (120) and the first side thickness measuring piece (130); the second low vacuum chamber (250) is located between the second side coating drum (210) and the second side thickness measuring piece (220); and a first auxiliary cooling roller (161) is arranged in the first low vacuum chamber (160), and a second auxiliary cooling roller (251) is arranged in the second low vacuum chamber (250).
5. The one-step forming current collector composite membrane preparation device according to claim 1, characterized in that: Each evaporation device (440) comprises an evaporation tank (441), a plurality of evaporation seats (442) are arranged in the evaporation tank (441), an evaporation boat (443) is clamped on the evaporation seat (442), and the step of the evaporation seat (442) is parallel to the evaporation boat (443), and the plurality of evaporation boats (443) are evenly arranged corresponding to the lateral width of the base film (600).
6. The one-step forming current collector composite membrane preparation device according to claim 1, characterized in that: A baffle plate (1210) is arranged in the winding chamber (1200), and the baffle plate (1210) is located below a plurality of first side coating drums (120) and a plurality of second side coating drums (210). A plurality of coating drum grooves (1210) are arranged on the baffle plate (1210), and the bottoms of the plurality of first side coating drums (120) are exposed to the first evaporation chamber (410) through the plurality of coating drum grooves (1210), and the bottoms of the plurality of second side coating drums (210) are exposed to the second evaporation chamber (420) through the plurality of coating drum grooves (1210).
7. The one-step forming current collector composite membrane preparation device according to claim 6, characterized in that: A plurality of evaporation baffles (1220) located below the blocking plate (1210) are arranged in the winding chamber (1200), and an evaporation baffle (1220) is arranged on each evaporation device (440).
8. The one-step forming current collector composite membrane preparation device according to claim 5, characterized in that: The evaporation seat (442) has a width of 35-40 mm, a length of 30-50 mm, and a height of 30-50 mm; the evaporation boat (443) has a width of 35-40 mm, a length of 130-150 mm, and a center distance between two adjacent evaporation boats (443) of 40-50 mm.
9. According to the one-time formed current collector composite membrane preparation device according to claim 5, a plurality of wire feeding devices (450) are arranged on both sides of the evaporation tank (441), each evaporation boat (443) is equipped with a wire feeding device (450), and the wire feeding devices (450) are arranged alternately on the evaporation tank (441).
10. A coating method for preparing a one-step forming current collector composite membrane according to any one of claims 1 to 9, characterized in that: include: After placing the base film (600) on the unwinding roller (110), close the vacuum chamber (300), open the telescopic partition (430), and start vacuuming; simultaneously start the biasing devices in the multiple first side coating drums (120) and the multiple second side coating drums (210), then start the multiple evaporation devices (440) and the multiple wire feeding devices (450) in the first evaporation chamber (410) and the second evaporation chamber (420), start the winding roller (230), and the multiple flattening rollers (140) to transfer the base film (600); after the evaporation device (440) reaches a suitable temperature, perform evaporation; During the evaporation process, the controller obtains data fed back by a plurality of temperature measuring devices (460), a first side thickness measuring piece (130), and a second side thickness measuring piece (220), compares the data with a set evaporation temperature range and a preset film thickness, and adjusts the power output of the evaporation device (440) and the wire feeding speed of the wire feeding device (450) according to the comparison result.
Citation Information
Cited By
Roll-to-roll sputtering device capable of forming thin films on both sides of the substrate within a single chamber
KR102883936B1