Deuterium gas preparation method

By using the electrodes loaded with catalysts in the preparation of deuterium gas for electrolytic treatment, combined with drying and decomposition treatment, the problems of high energy consumption and low gas production in the prior art are solved, and low energy consumption and high efficiency deuterium gas are achieved Preparation effect.

CN118996440APending Publication Date: 2024-11-22SUZHOU JINHONG GAS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411085101.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing deuterium gas preparation methods have shortcomings such as high energy consumption, high risk, high HD content, and small gas production. In particular, electrolysis has defects in energy consumption and cannot effectively improve the purity and stability of deuterium gas.

Method used

After heavy water is used to add electrolyte after degassing, and electrolyte is performed through the electrode supported by the catalyst. Combined with drying, deoxidation and decomposition treatment, the catalyst includes elements such as gallium, cerium, iron, ruthenium, nickel, etc., and the electrode is graphite electrode rod. Under oxygen environment, the electrolyte is sodium carbonate, sodium bicarbonate, and disodium hydrogen phosphate. The electrolyte is added to heavy water at 3-5 wt%, the catalyst loading is 8-10 wt%, and the molar ratio of active elements is 0.5 :1:3.

Benefits of technology

It realizes fast and efficient preparation of deuterium gas with low energy consumption, improves the purity and gas production of deuterium gas, and reduces the risk and energy consumption of the preparation process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a deuterium gas preparation method, which comprises the following steps of: degassing heavy water, adding electrolyte, electrolyzing the heavy water by adopting an electrode to obtain deuterium gas, and drying, deoxidizing and purifying the deuterium gas to obtain the deuterium gas, the catalyst at least comprises at least two active elements of a gallium element, a cerium element, an iron element, a ruthenium element and a nickel element. The invention provides a brand-new technical means for preparing deuterium by electrolysis, so that the deuterium can be quickly and efficiently prepared with low energy consumption under the catalytic condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of deuterium gas preparation, and particularly relates to a method for preparing deuterium gas. Background Art

[0002] Deuterium gas is praised as the "natural fuel of the future" and is increasingly favored by researchers. Deuterium gas instruments have unique properties and are widely used. An important use of deuterium gas in national defense is as the raw material gas for deuterium fluoride laser weapons. Deuterium fluoride lasers use deuterium gas to react with nitrogen trifluoride and other materials to produce excited deuterium fluoride, which releases energy to produce laser beams during the transition back to the steady state. Deuterium fluoride lasers have the advantages of high energy, good beam quality, and good atmospheric transmission performance. They can be used as integrated anti-missile weapons for shipborne and land use. The improvement and stability of deuterium gas purity will have a significant impact on the quality of the laser beam, which can improve the light output efficiency, light output energy, light output stability and light output consistency of chemical lasers, and play a role in improving and improving the light output performance of deuterium fluoride chemical laser weapons. It plays an extremely important role in the future military development and the improvement of human living standards, and plays an irreplaceable role. At the same time, deuterium gas has broad application prospects in nuclear energy and controlled nuclear fusion reactions. It is also widely used in medical testing, pharmaceuticals, polymer material synthesis and modification, new light sources, agricultural breeding, neutron logging and scientific research.

[0003] At present, the existing methods for preparing deuterium gas include liquid hydrogen distillation, chromatography separation, laser excitation, heavy water electrolysis, etc. The first three methods have the disadvantages of high energy consumption, high risk, high HD (deuterated hydrogen) content, and low gas production. The existing electrolysis method has the disadvantages of high energy consumption, etc.

[0004] Therefore, in view of the above technical problems, it is necessary to provide a method for preparing deuterium gas.

[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing deuterium gas.

[0007] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:

[0008] The deuterium gas preparation method comprises the following steps: adding electrolyte to degas heavy water, electrolyzing the heavy water with electrodes to obtain deuterium gas, and drying, deoxidizing and removing impurities from the deuterium gas to obtain the deuterium gas. The electrodes are carbon rods with catalysts loaded on the surfaces thereof, and the catalysts include at least two active elements selected from gallium, cerium, iron, ruthenium and nickel.

[0009] In one or more embodiments of the present invention, the carbon rod is a graphite electrode rod obtained by anodizing with a high-voltage arc in an oxygen-rich environment.

[0010] In one or more embodiments of the present invention, the oxygen-rich environment is a nitrogen-oxygen mixed gas environment, wherein the oxygen content is not less than 30 v / v%.

[0011] In one or more embodiments of the present invention, the high voltage is 13000-15000V DC.

[0012] In one or more embodiments of the present invention, the arc duration is 2-3S.

[0013] In one or more embodiments of the present invention, the electrolyte is selected from: sodium carbonate, sodium bicarbonate, disodium hydrogen phosphate.

[0014] In one or more embodiments of the present invention, the electrolyte is added in an amount of 3-5 wt % in heavy water.

[0015] In one or more embodiments of the present invention, the catalyst is an active element supported by a porous carbon support.

[0016] In one or more embodiments of the present invention, the loading amount of active elements in the catalyst is 8-10 wt %.

[0017] In one or more embodiments of the present invention, the active elements are composed of gallium, cerium, and nickel in a molar ratio of 0.5:1:3.

[0018] Compared with the prior art, the deuterium gas preparation method of the present invention provides a new technical means for preparing deuterium by electrolysis, thereby realizing rapid and efficient preparation of deuterium with low energy consumption under catalytic conditions. DETAILED DESCRIPTION

[0019] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0020] Including but not limited to the following examples, the deoxygenation catalyst is prepared by the following method: 8g Pd(NH3)4Cl2, 3g (NH4)6Mo7O 24·4H2O was dissolved in deionized water to obtain an active component infiltration solution. 40g of porous alumina was added to the infiltration solution and stirred evenly. The solution was infiltrated for 12h. After infiltration, the solution was dried at 130℃ for 6h, calcined at 500℃ for 5h, and then activated by passing hydrogen at 400℃ for 12h.

[0021] The preparation method of the present invention comprises the following steps: degassing heavy water at 80°C for 20 minutes, adding electrolyte, electrolyzing the heavy water at 12V DC using an electrode loaded with a catalyst, drying the collected cathode gas to remove heavy water, then passing the gas into a deoxygenation catalyst for deoxygenation, and finally removing impurities through a molecular sieve to obtain deuterium gas.

[0022] The electrolyte is sodium carbonate, and the amount of the electrolyte used is 3-5wt% of heavy water. The electrolyte is dried at 160-180°C for 1-3h before use. During the drying and heavy water removal process, deuterium gas is processed through silica gel.

[0023] The electrode loaded with the catalyst is obtained by anodizing a graphite electrode rod in a nitrogen and oxygen mixed gas environment (wherein the oxygen content is not less than 30v / v%) by a DC 13000-15000V high voltage arc for 2-3s. The oxide of the catalyst active component is dispersed in anhydrous ethanol, and after being fully dispersed, the electrode rod is fully immersed for 2-6h and continuously ultrasonicated, and the electrode loaded with the catalyst is obtained after drying.

[0024] Example 1

[0025] The preparation method of this embodiment is to degas heavy water at 80°C for 20 minutes, then add electrolyte, electrolyze the heavy water at 12V DC using an electrode loaded with a catalyst, dry the collected cathode gas to remove heavy water, then pass it into a deoxygenation catalyst for deoxygenation, and finally remove impurities through a molecular sieve to obtain deuterium gas.

[0026] The electrolyte is sodium carbonate, and the amount of the electrolyte used is 3 wt % of heavy water. The electrolyte is dried at 160° C. for 3 hours before use. During the drying and deuterium removal process, deuterium gas is passed through silica gel for treatment.

[0027] The electrode loaded with the catalyst is: a graphite electrode rod with a diameter of 10 mm is anodized by a DC 13000V high voltage arc for 2S in a nitrogen and oxygen mixed gas environment (wherein the oxygen content is 30v / v%). The oxide of the catalyst active component is dispersed in anhydrous ethanol, and after being fully dispersed, the electrode rod is fully immersed for 2h and continuously ultrasonicated, and the electrode loaded with the catalyst is obtained after drying.

[0028] The single cathode deuterium gas production in this embodiment is 7.25 mL / h.

[0029] Example 2

[0030] The preparation method of this embodiment is different from that of Embodiment 1 only in that the amount of electrolyte used is 4 wt % of heavy water.

[0031] The single cathode deuterium gas production in this embodiment is 7.33 mL / h.

[0032] Example 3

[0033] The preparation method of this embodiment is different from that of Embodiment 1 only in that the amount of electrolyte used is 5 wt % of heavy water.

[0034] The single cathode deuterium gas production in this embodiment is 7.28 mL / h.

[0035] Example 4

[0036] The preparation method of this embodiment is different from that of Embodiment 2 only in that the electrolyte is sodium bicarbonate.

[0037] The single cathode deuterium gas production in this embodiment is 7.13 mL / h.

[0038] Example 5

[0039] The preparation method of this embodiment is different from that of Embodiment 2 only in that the electrolyte is disodium hydrogen phosphate.

[0040] The single cathode deuterium gas production in this embodiment is 5.95 mL / h.

[0041] Example 6

[0042] The preparation method of this embodiment is different from that of Embodiment 3 only in that the electrolyte is sodium bicarbonate.

[0043] The single cathode deuterium gas production in this embodiment is 7.58 mL / h.

[0044] Example 7

[0045] The preparation method of this embodiment is different from that of Embodiment 3 only in that the electrolyte is disodium hydrogen phosphate.

[0046] The single cathode deuterium gas production in this embodiment is 7.29 mL / h.

[0047] Example 8

[0048] The preparation method of this embodiment is different from that of embodiment 6 only in that: the electrode loaded with the catalyst is obtained by anodizing a graphite electrode rod by a DC 14000V high voltage arc for 2.3S in a nitrogen and oxygen mixed gas environment. The oxide of the catalyst active component is dispersed in anhydrous ethanol, and after being fully dispersed, the electrode rod is fully immersed for 4 hours and continuously ultrasonicated, and then dried to obtain the electrode loaded with the catalyst.

[0049] The single cathode deuterium gas production in this embodiment is 8.35 mL / h.

[0050] Example 9

[0051] The preparation method of this embodiment is different from that of embodiment 6 only in that: the electrode loaded with the catalyst is obtained by anodizing a graphite electrode rod in a nitrogen and oxygen mixed gas environment by a DC 15000V high voltage arc for 3S. The oxide of the catalyst active component is dispersed in anhydrous ethanol, and after being fully dispersed, the electrode rod is fully immersed for 6 hours and continuously ultrasonicated, and then dried to obtain the electrode loaded with the catalyst.

[0052] The single cathode deuterium gas production in this embodiment is 8.03 mL / h.

[0053] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0054] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing deuterium gas, characterized in that: include After degassing, electrolyte is added to heavy water, and electrodes are used to electrolyze heavy water to obtain deuterium gas, and the deuterium gas is dried, deoxidized, and impurity-removed to obtain deuterium gas. The electrode is a carbon rod with a catalyst loaded on the surface, and the catalyst includes at least two active elements of gallium, cerium, iron, ruthenium, and nickel.

2. The method for preparing deuterium gas according to claim 1, characterized in that: The carbon rod is obtained by anodizing a graphite electrode rod through a high-voltage arc in an oxygen-rich environment.

3. The method for preparing deuterium gas according to claim 2, characterized in that: The oxygen-rich environment is a nitrogen-oxygen mixed gas environment, wherein the oxygen content is not less than 30 v / v%.

4. The method for preparing deuterium gas according to claim 2, characterized in that: The high voltage is DC 13000-15000V.

5. The method for preparing deuterium gas according to claim 2, characterized in that: The arc duration is 2-3S.

6. The method for preparing deuterium gas according to claim 1, characterized in that: The electrolyte is selected from the group consisting of sodium carbonate, sodium bicarbonate, and disodium hydrogen phosphate.

7. The method for preparing deuterium gas according to claim 6, characterized in that: The electrolyte is added in an amount of 3-5 wt % in heavy water.

8. The method for preparing deuterium gas according to claim 1, characterized in that: The catalyst is an active element supported by a porous carbon carrier.

9. The method for preparing deuterium gas according to claim 8, characterized in that: The loading amount of active elements in the catalyst is 8-10 wt%.