Preparation method and application of CoFeCrLDHFeOOH heterostructure

By growing CoFeCrLDHFeOOH heterostructure on foam nickel and combining ultrasonic technology, the problems of high cost of precious metal catalysts and poor stability of non-precious metals are solved, and low-cost and efficient electrocatalytic oxygen evolution performance and long-term stable operation are achieved.

CN118996501APending Publication Date: 2024-11-22PINGGAO GRP ENERGY STORAGE TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411053923.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The cost of precious metal catalysts is high and scarce, the stability of non-precious metal catalysts is poor, and bubble adhesion in the electrocatalytic oxygen evolution reaction affects the activity and stability, limiting the industrial application of electrolytic water technology.

Method used

The CoFeCrLDHFeOOH heterostructure is used as an electrocatalyst to grow nano-flake-like structures in situ on nickel foam through hydrothermal reaction, and combined with ultrasonic technology, the activity and stability of the catalyst are improved.

Benefits of technology

A low-cost and high-stability electrocatalyst is achieved, which significantly improves oxygen evolution performance and reduces overpotentially. The electrocatalyst remains efficient during long-term operation and has excellent cycling durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996501A_ABST
    Figure CN118996501A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method and application of a CoFeCrLDHFeOOH heterostructure, and belongs to the technical field of electrocatalysis. Then adding Co (NO3) 2.6 H2O, Fe (NO3) 3.9 H2O, Cr (NO3) 3.9 H2O and urea in different molar ratios into water, stirring to a transparent state, introducing argon to a saturated state, and then adding NH4F to obtain a transparent gray solution; carrying out hydrothermal reaction on the foamed nickel and the transparent gray solution; and finally, the foamed nickel is cleaned and dried, a CoFeCr LDH / FeOOH material growing on the foamed nickel in situ is obtained, and CoFeCr LDH / FeOOH / NF is formed. According to the present invention, the synthesis method is simple, the cost is low, the active area and the intrinsic activity are high, the stability is high, the overpotential change is small, and the cycle durability is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrocatalysis, and in particular relates to a preparation method and application of a CoFeCrLDHFeOOH heterostructure. Background Art

[0002] In the past few decades, the increasingly serious environmental and energy crises have accelerated the transition from traditional fossil fuel energy to environmentally friendly renewable resources. Hydrogen has a huge energy density (142 MJ kg -1 ) and as one of the few carbon-free energy carriers, it is widely considered to be a very promising alternative to replace fossil fuels in the future.

[0003] Electrochemical water splitting is one of the most promising technologies for developing sustainable energy storage and conversion systems. Water splitting is divided into two half reactions: hydrogen evolution reaction (HER) and oxygen evolution reaction (OER). Since the number of electrons involved in oxygen evolution is twice that of hydrogen evolution, the overpotential of oxygen evolution is often higher than that of hydrogen evolution. Therefore, the efficiency of full water splitting is mainly limited by the slow reaction kinetics of oxygen evolution reaction. The efficiency of electrocatalysis is mainly determined by the characteristics of the electrocatalyst itself, so a suitable catalyst is crucial.

[0004] Although noble metal-based catalysts have high OER activity, for example, iridium and ruthenium are widely considered to be the best OER electrocatalysts in alkaline environments, the high cost and scarcity of noble metals hinder the large-scale use of water electrolysis technology and pose a challenge to the industrialization of water electrolysis technology. On the other hand, the stability of most non-noble metal-based catalysts is too poor, which is also one of the reasons that hinder commercialization. In addition, a large number of bubbles will be generated during the gas evolution process. Once these bubbles attach to the catalyst surface, they will have an adverse effect on the activity and stability of the catalyst, not only blocking the electrochemical active sites and hindering effective mass transfer, but also leading to a significant increase in the ohmic overpotential and concentration overpotential. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing a CoFeCrLDHFeOOH heterostructure and application thereof.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a CoFeCrLDHFeOOH heterostructure, comprising the following steps: S1. Soak the nickel foam in a H2SO4 solution with a concentration of 0.8 to 1.2 mol / L for 20 to 30 min, take it out and soak it in ultrapure water and anhydrous ethanol for 10 min each, and then place it in a vacuum drying oven for vacuum drying for 2 h to complete the pretreatment of the nickel foam; S2. Add different molar ratios of Co(NO3)2·6H2O, Fe(NO3)3·9H2O, Cr(NO3)3·9H2O and 2.5mmol urea to 20mL water, stir until transparent and pass argon to saturation, then add 2mmol NH4F, stir for 30min and pass argon to saturation to obtain a transparent gray solution; S3, adding the nickel foam pretreated in step S1 and the transparent gray solution obtained in step S2 into a reactor, and then placing the reactor in a blast drying oven, controlling the temperature of the blast drying oven to rise to 140-160° C. and maintaining the temperature for 10-14 hours, so that a hydrothermal reaction occurs in the reactor; S4. After the reactor was naturally cooled, the reddish-brown nickel foam was taken out and washed three times with water and anhydrous ethanol respectively, and then dried at 60°C under vacuum conditions for 8-10 hours. Finally, the CoFeCrLDH / FeOOH material in situ grown on the nickel foam was obtained, namely CoFeCr LDH / FeOOH / NF.

[0007] Further, in step S2, the Fe content is 10%-50%; the ratio of Co to Cr is maintained at 1:1; and the total amount of metal ions is 1.2 mmol.

[0008] Another object of the present invention is to provide an application of CoFeCr LDH / FeOOH / NF obtained by a method for preparing a CoFeCrLDHFeOOH heterostructure in electrocatalytic oxygen evolution, comprising the following steps: S100, preparing a 1.0 M potassium hydroxide solution as an electrocatalytic electrolyte, and introducing nitrogen to remove air; S200, CoFeCr LDH / FeOOH / NF was used as the working electrode, graphite as the counter electrode, and saturated calomel electrode as the reference electrode, connected to an electrochemical workstation, and an electrocatalytic oxygen evolution reaction was carried out in the electrolyte; S300, adding ultrasound during the electrocatalytic oxygen evolution reaction.

[0009] Further, in step S300, the temperature of the electrolyte is stabilized at 25±2°C during the ultrasonic process.

[0010] The beneficial effects of the present invention are: (1) The present invention successfully prepared the CoFeCr LDH / FeOOH heterostructure by controlling the content of iron salt, obtained the CoFeCr LDH / FeOOH material grown in situ on nickel foam, and formed the non-precious catalyst CoFeCr LDH / FeOOH / NF. The method is simple and low-cost.

[0011] (2) The present invention synthesized a three-dimensional catalyst CoFeCr LDH / FeOOH / NF with a nanosheet flower-like structure, which has a higher active area and intrinsic activity. In addition, the structure has higher stability, is not easy to agglomerate compared to the tubular nanowire structure, and is simpler to synthesize.

[0012] (3) The present invention combines electrochemistry with ultrasound, using ultrasound to significantly improve the oxygen evolution performance of the CoFeCr LDH / FeOOH / NF electrocatalyst and explores the mechanism of ultrasound-enhanced electrocatalysis. The study found that ultrasound can effectively promote the detachment of bubbles from the surface of CoFeCr LDH / FeOOH / NF, promote the formation of high-valent metals, promote reconstruction, and improve activity.

[0013] (4) In alkaline solution, the overpotential of CoFeCr LDH / FeOOH / NF electrocatalyst as a working electrode is low, and the application of ultrasound makes its overpotential further decrease. Its performance is better than most reported electrocatalysts. This electrocatalyst can be used as a working electrode at 50 mA·cm -2 It can operate stably for at least 100 hours at a stable current density with little overpotential change and has excellent cycle durability. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] The present invention will be described in detail below with reference to the accompanying drawings and in combination with examples, and the advantages and implementation methods of the present invention will become more obvious. The contents shown in the accompanying drawings are only used to explain the present invention and do not constitute any limitation to the present invention in any sense. In the accompanying drawings: Figure 1 1 is the XRD spectrum of CoFeCr LDH / FeOOH and CoFeCr LDH with different Fe contents in the present invention.

[0015] Figure 2 It is a low-magnification scanning electron microscope image of CoFeCr LDH / FeOOH / NF-1 of the present invention.

[0016] Figure 3 The linear sweep voltammetry curves of CoFeCr LDH / FeOOH / NF with different Fe contents and its comparative sample in the oxygen evolution reaction of electrolyzed water are shown in FIG.

[0017] Figure 4 The linear sweep voltammetry curves of CoFeCr LDH / FeOOH / NF-1 of the present invention with and without ultrasonic waves are shown.

[0018] Figure 5 This is a graph showing the overpotential variation of CoFeCr LDH / FeOOH / NF-1 in the electrolytic water oxygen evolution reaction of the present invention.

[0019] Figure 6 This is an XPS analysis chart of the ultrasonic wave promoting the formation of high-valent metals in the present invention. DETAILED DESCRIPTION

[0020] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the best embodiment.

[0021] A method for preparing a CoFeCrLDHFeOOH heterostructure comprises the following steps: S1. Soak a certain area of ​​nickel foam in a H2SO4 solution with a concentration of 0.8-1.2 mol / L for 20-30 min, take it out and soak it in ultrapure water and anhydrous ethanol for 10 min each, then place it in a vacuum drying oven for vacuum drying for 2 h to complete the pretreatment of nickel foam.

[0022] S2. Add different molar ratios of Co(NO3)2·6H2O, Fe(NO3)3·9H2O, Cr(NO3)3·9H2O and 2.5mmol urea to 20mL water, stir until transparent and pass argon to saturation. Then add 2mmol NH4F, stir for 30min and pass argon to saturation to obtain a transparent gray solution.

[0023] Among them, the Fe content is 10%-50%; the ratio of Co and Cr is maintained at 1:1; and the total amount of metal ions is 1.2 mmol.

[0024] The optimal ratio of Co to Cr is 1:1. The performance of the present invention is optimal under this ratio. At the same time, the variables can be reduced to facilitate observation of the effect of Fe content changes on the performance of the present invention. Too little Fe content will result in an insignificant doping effect. When the Fe content exceeds 10%, the OER performance will be significantly enhanced; when the Fe content exceeds 50%, the CoFeCrLDH phase will be reduced, and the OER performance will decrease instead.

[0025] S3, adding the nickel foam pretreated in step S1 and the transparent gray solution obtained in step S2 into a reactor, and then placing the reactor in a forced air drying oven, controlling the temperature of the forced air drying oven to rise to 140-160° C. and maintaining the temperature for 10-14 hours, so that a hydrothermal reaction occurs in the reactor.

[0026] Among them, since NH4F is added to the transparent gray solution obtained in step S2, not only the morphology can be controlled to eventually form a nanostructure, but also the nickel foam can be etched, so that the transparent gray solution and the nickel foam are more closely combined.

[0027] S4. After the reactor was naturally cooled, the reddish-brown nickel foam was taken out and washed three times with water and anhydrous ethanol respectively, and then dried at 60°C under vacuum conditions for 8-10 hours. Finally, the CoFeCrLDH / FeOOH material in situ grown on the nickel foam was obtained, namely CoFeCr LDH / FeOOH / NF.

[0028] Among them, according to the content of added Fe ions, CoFeCr LDH / FeOOH is marked from large to small as CoFeCr LDH / FeOOH-1, CoFeCr LDH / FeOOH-2, CoFeCr LDH / FeOOH-3, etc.

[0029] Another object of the present invention is to provide an application of CoFeCr LDH / FeOOH / NF obtained by a method for preparing a CoFeCrLDHFeOOH heterostructure in electrocatalytic oxygen evolution, comprising the following steps: S100, preparing a 1.0 M potassium hydroxide solution as an electrocatalytic electrolyte, and introducing nitrogen to remove air; S200, CoFeCr LDH / FeOOH / NF was used as the working electrode, graphite as the counter electrode, and saturated calomel electrode as the reference electrode, connected to an electrochemical workstation, and an electrocatalytic oxygen evolution reaction was carried out in the electrolyte; S300, using a KH-100 ultrasonic cleaning machine to add ultrasound during the electrocatalytic oxygen evolution reaction.

[0030] The temperature of the electrolyte was stabilized at 25±2°C during the ultrasonic process.

[0031] like Figure 1 As shown, the ordinate is the intensity of XRD (X-ray diffraction), the abscissa is twice the angle of X-ray incidence (2θ), and the CoFeCr LDH / FeOOH with different Fe contents are CoFeCr LDH / FeOOH-1 and CoFeCr LDH / FeOOH-2, CoFeCr LDH / FeOOH-1, CoFeCr LDH / FeOOH-2, and the molar ratios of the metal feed materials Co(NO3)2·6H2O, Fe(NO3)3·9H2O, and Cr(NO3)3·9H2O in CoFeCr LDH are 1:2:1, 1:1:1, and 2:1:2, respectively. PDF#46-0605 and PDF#75-1594 are the standard cards of Co LDH and FeOOH, respectively. Co LDH and FeOOH appear in the XRD graph, indicating that Fe and Cr are successfully incorporated into Co LDH, and a CoFeCr LDH / FeOOH heterogeneous structure appears.

[0032] like Figure 2As shown, the microstructure of CoFeCr LDH / FeOOH / NF-1 is a nanoflower ball composed of nanosheets, wherein the molar ratio of the metal feeds Co(NO3)2·6H2O, Fe(NO3)3·9H2O, and Cr(NO3)3·9H2O in CoFeCr LDH / FeOOH / NF-1 is 1:2:1.

[0033] like Figure 3 As shown, the ordinate is the current density during the electrolysis of water for oxygen evolution, and the abscissa is the voltage during the electrolysis of water for oxygen evolution. The figure shows the oxygen evolution LSV curves of CoFeCr LDH / FeOOH / NF-1, CoFeCr LDH / FeOOH / NF-2, CoFeCr LDH / NF, nickel foam (NF), and commercial ruthenium oxide (RuO2). Among them, the molar ratios of the metal feeds Co(NO3)2·6H2O, Fe(NO3)3·9H2O, and Cr(NO3)3·9H2O in CoFeCr LDH / FeOOH / NF-1, CoFeCr LDH / FeOOH / NF-2, and CoFeCr LDH / NF are 1:2:1, 1:1:1, and 2:1:2, respectively.

[0034] CoFeCr LDH / FeOOH / NF-1, CoFeCr LDH / FeOOH / NF-2, CoFeCr LDH / NF, NF, RuO2 at 50mA·cm -2 The overpotentials at 235 mV, 262 mV, 284 mV, 338 mV, and 330 mV are respectively. It is not difficult to see that CoFeCr LDH / FeOOH / NF-1 has the lowest overpotential. The incorporation of Fe and Cr leads to the oxygen evolution performance of LDH being better than that of commercial ruthenium oxide, and as the Fe content further increases, the CoFeCr LDH / FeOOH heterostructure is generated, and the performance is further enhanced.

[0035] like Figure 4 As shown in the figure, the electrolytic cell was placed in an ultrasonic cleaning machine to test the oxygen evolution performance of CoFeCrLDH / FeOOH-1 when ultrasound was turned on and off. After applying ultrasound, CoFeCr LDH / FeOOH / NF-1 -2 The overpotential at the current density of 1.34 V was reduced by 8 mV.

[0036] like Figure 5 As shown in the figure, the ordinate is the voltage of water electrolysis and the abscissa is time. The stability of CoFeCr LDH / FeOOH-1 under long-term operation is tested by observing the amplitude of voltage change over time. -2It operated stably for at least 100 hours at a stable current density of 1.5 Å, with an overpotential change of only 16 mV.

[0037] It can be seen that the present invention successfully prepared the CoFeCr LDH / FeOOH heterostructure by controlling the content of Fe salt, and the method is simple and low in cost.

[0038] The present invention synthesizes a three-dimensional catalyst-CoFeCr LDH / FeOOH / NF with a nanosheet flower-like structure, which has a higher active area and intrinsic activity, and the structure makes it have higher stability.

[0039] The present invention combines electrochemistry with ultrasound, utilizes ultrasound to significantly improve the oxygen evolution performance of CoFeCr LDH / FeOOH / NF electrocatalyst and explores the mechanism of ultrasound-enhanced electrocatalysis. The study found (through X-ray photoelectron spectroscopy technology) that ultrasound can promote the detachment of bubbles from the electrode surface and the formation of high-valent metals, thereby improving activity.

[0040] like Figure 6 As shown in Figure 2, in order to clarify the reason why the CoFeCr LDH / FeOOH / NF electrocatalyst has excellent OER performance, the CoFeCr LDH / FeOOH / NF-1 samples after OER and ultrasonic OER were collected and analyzed by XPS. 3 / 2 Peak and Cr 2p 3 / 2 The peak splits into two peaks, at Co 2p 3 / 2 In the spectrum of 3+ Cr 6+ appears at 579.0 eV, indicating that the Cr ions are partially oxidized to a higher valence state. Compared with the sample after OER, the Co 3+ and Cr 6+ The content of ions increased and the peak position shifted to the direction of higher binding energy. This shows that ultrasound can promote the generation of high-valent metal ions and change the electronic structure.

[0041] In alkaline solution, the CoFeCr LDH / FeOOH / NF electrocatalyst exhibited a high conductivity at 50 mA·cm -2 The overpotential required is only 235 mV, and the application of ultrasound reduces its overpotential by 8 mV. Its performance is better than most reported electrocatalysts. The electrode can be used at 50 mA cm -2 The overpotential changed by only 16 mV and the stable current density was maintained for at least 100 hours. (at 10mA·cm -2The overpotential increased by only 14 mV during a 100-h long cycle at a current density of 1.5 Å (Figure 2), demonstrating excellent cycling durability.

[0042] The embodiments of the present invention are described in detail above, but the contents are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the present invention.

Claims

1. A method for preparing a CoFeCrLDHFeOOH heterostructure, Features: The following steps are involved: S1. Place the nickel foam in a H solution with a concentration of 0.8 to 1.2 mol / L. 2 SO 4 The nickel foam is immersed in a solution, taken out and immersed in ultrapure water and anhydrous ethanol for ultrasonic treatment respectively, and then vacuum dried to complete the pretreatment of the nickel foam; S2, different molar ratios of Co(NO 3 ) 2 6H 2 O,Fe(NO 3 ) 3 9H 2 O,Cr(NO 3 ) 3 9H 2 O and urea were added to the water, stirred until transparent and argon was introduced to saturation, followed by addition of NH 4 F, stirring and introducing argon to saturation to obtain a transparent gray solution; S3, adding the nickel foam pretreated in step S1 and the transparent gray solution obtained in step S2 into a reactor, and then placing the reactor in a blast drying oven, heating it and keeping it for a period of time to allow a hydrothermal reaction to occur in the reactor; S4. After the reactor is cooled naturally, the reddish-brown nickel foam is taken out, and it is washed with water and anhydrous ethanol respectively, and then dried under vacuum conditions to obtain a CoFeCr LDH / FeOOH material grown in situ on the nickel foam, forming CoFeCrLDH / FeOOH / NF.

2. The method for preparing the CoFeCrLDHFeOOH heterostructure according to claim 1, Features: In step S1, the nickel foam is placed in a H 2 SO 4 The samples were soaked in the solution for 20 to 30 minutes, taken out and soaked in ultrapure water and anhydrous ethanol for 10 minutes each, and then placed in a vacuum drying oven for vacuum drying for 2 hours.

3. The method for preparing the CoFeCrLDHFeOOH heterostructure according to claim 1, Features: In step S2, different molar ratios of Co(NO 3 ) 2 6H 2 O,Fe(NO 3 ) 3 9H 2 O,Cr(NO 3 ) 3 9H 2 O and 2.5 mmol urea were added to 20 mL water, stirred until transparent and argon was introduced to saturation, followed by the addition of 2 mmol NH 4 F, stir for 30 min and introduce argon until saturated.

4. The method for preparing the CoFeCrLDHFeOOH heterostructure according to claim 1, Features: In step S2, the Fe content is 10%-50%; the ratio of Co to Cr is maintained at 1:1; and the total amount of metal ions is 1.2 mmol.

5. The method for preparing the CoFeCrLDHFeOOH heterostructure according to claim 1, Features: In step S3, the temperature of the blast drying oven is controlled to rise to 140-160°C and maintained at this temperature for 10-14 hours.

6. The method for preparing the CoFeCrLDHFeOOH heterostructure according to claim 1, Features: In step S4, the reddish-brown nickel foam is washed three times with water and three times with anhydrous ethanol, and then dried under vacuum at 60° C. for 8 to 10 hours.

7. Use of CoFeCr LDH / FeOOH / NF obtained by the method for preparing the CoFeCrLDHFeOOH heterostructure according to any one of claims 1 to 6 in electrocatalytic oxygen evolution, Features: The following steps are involved: S100, using potassium hydroxide solution as an electrocatalytic electrolyte, and introducing nitrogen to remove air; S200, CoFeCr LDH / FeOOH / NF was used as the working electrode, graphite as the counter electrode, and saturated calomel electrode as the reference electrode, connected to an electrochemical workstation, and an electrocatalytic oxygen evolution reaction was carried out in the electrolyte; S300, adding ultrasound during the electrocatalytic oxygen evolution reaction to achieve electrocatalytic oxygen evolution.

8. Application of CoFeCr LDH / FeOOH / NF obtained by the method for preparing CoFeCrLDHFeOOH heterostructure according to claim 7 in electrocatalytic oxygen evolution, Features: In step 100, the potassium hydroxide solution is 1.0M.

9. Application of CoFeCr LDH / FeOOH / NF obtained by the method for preparing CoFeCrLDHFeOOH heterostructure according to claim 7 in electrocatalytic oxygen evolution, Features: In step S300, the temperature of the electrolyte is stabilized at 25±2°C during the ultrasonication process.