Nickel hydroxide coated copper dendrite electrocatalyst and preparation method thereof

By using a copper dendrite electrocatalyst coated with nickel hydroxide in electrolytic hydrogen production, the problem of limited oxygen evolution reaction rate in the traditional electrolytic hydrogen production method is solved, and high-efficiency formaldehyde oxidation and hydrogen production under normal temperature and pressure is achieved. , demonstrates excellent electrocatalytic performance and stability.

CN118996503AActive Publication Date: 2024-11-22ZHEJIANG UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411071212.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-22
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

In the traditional electrolytic hydrogen production method, the four electron transfer process and high theoretical potential of the oxygen evolution reaction limit the hydrogen production rate, and the mixing of hydrogen and oxygen with the product can easily cause explosions, limiting commercial application; the oxidation reaction of small molecules of organic matter is thermodynamic. It has more advantages, but there are still problems such as high tank pressure and high hydrogen production and high power consumption.

Method used

The copper dendrite electrocatalyst coated with nickel hydroxide is prepared by a two-step electrodeposition method. The first step is to electrodeposit copper dendrite in acidic copper sulfate solution, and the second step is to electrodeposit nickel hydroxide in nickel sulfate solution. A copper dendrite electrocatalyst coated with nickel hydroxide is formed for formaldehyde oxidation reaction.

Benefits of technology

Under normal temperature and pressure, the nickel hydroxide-coated copper dendrite electrocatalyst exhibits excellent formaldehyde oxidation hydrogen production performance and stability, and can efficiently produce hydrogen at ultra-low potential, with high application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996503A_ABST
    Figure CN118996503A_ABST
Patent Text Reader

Abstract

The invention relates to a nickel hydroxide coated copper dendrite electrocatalyst, which is prepared by the following method: soaking a piece of foamy copper in a hydrochloric acid solution, removing a surface oxide layer, washing with water and ethanol, and drying; the foamy copper substrate is placed in a copper sulfate solution, a saturated calomel electrode serves as a reference electrode, a carbon rod serves as a counter electrode, foamy copper serves as a working electrode, electro-deposition is carried out under the voltage of-1.2 V to-1.0 V, and copper dendrite loaded foamy copper is obtained after water washing; the preparation method comprises the following steps: placing copper dendrites in a nickel nitrate solution, taking a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode and foamy copper as a working electrode, carrying out electrodeposition under-1.1 to-0.9 V, washing with water, and drying to obtain the nickel hydroxide coated copper dendrite electrocatalyst, the invention further provides a preparation method of the nickel hydroxide coated copper dendrite electrocatalyst. The preparation process is simple, the reaction time is short, and the material prepared at normal temperature and normal pressure has excellent formaldehyde oxidation hydrogen production performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a nickel hydroxide-coated copper dendrite electrocatalyst and a preparation method thereof. The catalyst can be used for research on formaldehyde oxidation hydrogen production reaction. Background Art

[0002] As an important chemical industrial raw material and zero-carbon energy carrier, hydrogen has a wide range of applications in the industrial and energy fields. Among the many hydrogen production methods, water electrolysis is considered to be one of the most effective methods for large-scale hydrogen production. Traditional water electrolysis consists of a hydrogen evolution reaction at the cathode and an oxygen evolution reaction at the anode. However, the four-electron transfer process and high theoretical potential (1.23V) involved in the oxygen evolution reaction result in the water electrolysis rate being generally limited by the oxygen evolution reaction rate. In addition, the oxygen product of oxygen evolution is cheap, and it is easy to cause explosions when mixed with hydrogen, which seriously limits the commercial application of water electrolysis to produce hydrogen.

[0003] Compared with oxygen evolution, the small molecule oxidation reaction of organic matter has more thermodynamic advantages. It can not only avoid the mixing of H2 and O2, but also realize the value-added of organic matter. Replacing the oxygen evolution reaction with the small molecule oxidation reaction of organic matter can greatly improve the efficiency of hydrogen production by water electrolysis, but there are still problems such as high cell pressure and high power consumption for hydrogen production.

[0004] The formaldehyde oxidation reaction can be carried out at an ultra-low potential (<0.1V), while producing value-added products such as formic acid and hydrogen at the anode. It is one of the best choices to replace the oxygen evolution reaction. Copper-based catalysts can achieve formaldehyde oxidation at ultra-low potentials, and compared with precious metal catalysts, copper-based catalysts are inexpensive, so they are considered to be the best materials for anodic formaldehyde oxidation reactions. In order to further improve the performance of copper-based catalysts in formaldehyde oxidation reactions, adjusting the structure and composition of the catalyst is an effective strategy. Summary of the invention

[0005] In order to overcome the shortcomings of the prior art, the present invention relates to a nickel hydroxide-coated copper dendrite electrocatalyst for catalyzing formaldehyde oxidation to produce hydrogen and a preparation method thereof, as well as research on its electrocatalytic hydrogen evolution performance. The preparation process is simple and the reaction time is short. The material prepared at room temperature and pressure has excellent formaldehyde oxidation to produce hydrogen performance.

[0006] The technical solution adopted by the present invention is:

[0007] A nickel hydroxide-coated copper dendrite electrocatalyst is prepared by the following method:

[0008] (1) Take a piece of 1-4 cm 2 The foamed copper was immersed in a 1-6M hydrochloric acid solution for 5-30 minutes to remove the surface oxide layer, washed with water and ethanol and then dried;

[0009] (2) placing the copper foam substrate in a 0.1-0.3M copper sulfate solution, using a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and copper foam as a working electrode, electroplating for 100-300 seconds at -1.2--1.0V, and washing with water to obtain copper dendrite-loaded copper foam;

[0010] (3) The copper dendrites are placed in a 0.1-0.2M nickel nitrate solution, with a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and a copper foam as a working electrode. The copper dendrites are electrodeposited at -1.1 to -0.9V for 50 to 150 seconds, washed with water, and dried to obtain a nickel hydroxide-coated copper dendrite electrocatalyst.

[0011] In the present invention, a typical nickel hydroxide-coated copper dendrite electrocatalyst is prepared by a two-step electrodeposition method. The first step is to electrodeposit copper dendrites in an acidic copper sulfate solution, and the second step is to electrodeposit nickel hydroxide in a nickel sulfate solution to form a nickel hydroxide-coated copper dendrite electrocatalyst.

[0012] A method for preparing a nickel hydroxide-coated copper dendrite electrocatalyst, the method comprising the following steps:

[0013] (1) Take a piece of 1-4 cm 2 The foamed copper was immersed in a 1-6M hydrochloric acid solution for 5-30 minutes to remove the surface oxide layer, washed with water and ethanol and then dried;

[0014] (2) placing the copper foam substrate in a 0.1-0.3M copper sulfate solution, using a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and copper foam as a working electrode, electroplating for 100-300 seconds at -1.2--1.0V, and washing with water to obtain copper dendrite-loaded copper foam;

[0015] (3) The copper dendrites are placed in a 0.1-0.2M nickel nitrate solution, with a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and a copper foam as a working electrode. The copper dendrites are electrodeposited at -1.1 to -0.9V for 50 to 150 seconds, washed with water, and dried to obtain a nickel hydroxide-coated copper dendrite electrocatalyst.

[0016] Furthermore, the concentration of copper sulfate and nickel nitrate, the potential and time of electrodeposition are regulated to control the morphology and structure of the material.

[0017] Preferably, the thickness of the nickel hydroxide is 5 to 7 nm.

[0018] The formaldehyde oxidation performance test is carried out at normal temperature and pressure. The specific operation process is as follows:

[0019] 1) The cutting area is 1×1~2×2cm 2The nickel hydroxide-coated copper dendrites were used as the working electrode, the Hg / HgO electrode was used as the reference electrode, and the graphite rod was used as the counter electrode.

[0020] 2) The performance test of formaldehyde oxidation and hydrogen production was carried out in an H-type electrolytic cell. One side of the electrolytic cell was composed of a working electrode and a reference electrode to form the anode of the electrolytic cell, and the other side was composed of a counter electrode to form the cathode of the electrolytic cell. The anolyte was a 0.1-1M KOH solution containing 0.1-0.5M formaldehyde, and the catholyte was a 0.1-1M KOH solution. The test procedures of linear scanning cyclic voltammetry and chronoamperometry were selected, and the current of the working electrode at different potentials was monitored by a computer. Then, the concentration of formaldehyde in the electrolyte after the electrolytic reaction was calculated using a UV-visible spectrophotometer and a standard curve of formaldehyde, the amount of hydrogen produced was calculated using the water displacement method, and the conversion rate and Faraday efficiency of the catalyst were calculated.

[0021] The beneficial effects of the present invention are mainly reflected in:

[0022] (1) We successfully prepared nickel hydroxide-coated copper dendrite electrocatalysts by a two-step electrodeposition method and demonstrated their application in formaldehyde oxidation to produce hydrogen.

[0023] (2) Nickel hydroxide-coated copper dendrite electrocatalyst exhibits excellent electrocatalytic performance and stability in the formaldehyde oxidation hydrogen production reaction and has high application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 These are the SEM and TEM images of the copper dendrite electrocatalyst coated with nickel hydroxide according to the specific embodiment 1 of the present invention.

[0025] Figure 2 This is a contact angle diagram of the copper dendrite electrocatalyst coated with nickel hydroxide according to specific embodiment 1 of the present invention.

[0026] Figure 3 This is the Raman image of the copper dendrite electrocatalyst coated with nickel hydroxide according to the specific embodiment 1 of the present invention.

[0027] Figure 4 This is the XRD diagram of the copper dendrite electrocatalyst coated with nickel hydroxide according to the specific embodiment 1 of the present invention.

[0028] Figure 5 This is the XPS graph of the copper dendrite electrocatalyst coated with nickel hydroxide according to the specific example 1 of the present invention.

[0029] Figure 6 This is the linear sweep voltammetry curve of the copper dendrite electrocatalyst coated with nickel hydroxide according to the specific example 1 of the present invention.

[0030] Figure 7This is a performance diagram of formaldehyde oxidation and hydrogen production of the nickel hydroxide-coated copper dendrite electrocatalyst in specific embodiment 1 of the present invention.

[0031] Figure 8 This is a stability performance diagram of the copper dendrite electrocatalyst coated with nickel hydroxide according to specific embodiment 1 of the present invention.

[0032] Fig. 9 This is the double layer capacitance curve of the copper dendrite electrocatalyst coated with nickel hydroxide according to the specific example 1 of the present invention.

[0033] Fig.10 This is a SEM image of the copper dendrite electrocatalyst coated with nickel hydroxide according to specific example 2 of the present invention.

[0034] Fig.11 This is the linear sweep voltammetry curve of the copper dendrite electrocatalyst coated with nickel hydroxide according to the specific example 2 of the present invention.

[0035] Fig.12 This is a SEM image of the copper dendrite electrocatalyst coated with nickel hydroxide according to specific example 3 of the present invention.

[0036] Fig.13 This is the linear sweep voltammetry curve of the copper dendrite electrocatalyst coated with nickel hydroxide according to the specific example 3 of the present invention.

[0037] Fig.14 This is a SEM image of the copper dendrite electrocatalyst coated with nickel hydroxide according to specific example 4 of the present invention.

[0038] Fig.15 This is the linear sweep voltammetry curve of the copper dendrite electrocatalyst coated with nickel hydroxide according to the specific example 4 of the present invention. DETAILED DESCRIPTION

[0039] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto:

[0040] Reference Figures 1 to 8 , a nickel hydroxide-coated copper dendrite electrocatalyst prepared by the following method:

[0041] (1) Take a piece of 1-4 cm 2 The foamed copper was immersed in a 1-6M hydrochloric acid solution for 5-30 minutes to remove the surface oxide layer, washed with water and ethanol and then dried;

[0042] (2) placing the copper foam substrate in a 0.1-0.3M copper sulfate solution, using a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and copper foam as a working electrode, electroplating for 100-300 seconds at -1.2--1.0V, and washing with water to obtain copper dendrite-loaded copper foam;

[0043] (3) The copper dendrites are placed in a 0.1-0.2M nickel nitrate solution, with a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and a copper foam as a working electrode. The copper dendrites are electrodeposited at -1.1 to -0.9V for 50 to 150 seconds, washed with water, and dried to obtain a nickel hydroxide-coated copper dendrite electrocatalyst.

[0044] The hydrogen evolution performance test of the nickel hydroxide-coated copper dendrite electrocatalyst of this embodiment was carried out on a CHI 660E electrochemical workstation, and the operation process was as follows:

[0045] 1) The cutting area is 1×1~2×2cm 2 The nickel hydroxide-coated copper dendrites were used as the working electrode, the Hg / HgO electrode was used as the reference electrode, and the graphite rod was used as the counter electrode.

[0046] 2) The performance test of formaldehyde oxidation and hydrogen production is carried out in an H-type electrolytic cell. One side of the electrolytic cell is the working electrode and the reference electrode forming the anode of the electrolytic cell, and the other side is the counter electrode forming the cathode of the electrolytic cell. The anolyte is a 0.1-1M KOH solution containing 0.1-0.5M formaldehyde, and the cathode electrolyte is a 0.1-1M KOH solution. The test procedures of linear scanning cyclic voltammetry and chronoamperometry are selected, and the current of the working electrode at different potentials is monitored by a computer. Then, the concentration of formaldehyde in the electrolyte after the electrolytic reaction is calculated using a UV-visible spectrophotometer and a standard curve of formaldehyde, the amount of hydrogen produced is calculated using the water displacement method, and the conversion rate and Faraday efficiency of the catalyst are calculated.

[0047] Example 1

[0048] A method for preparing a nickel hydroxide-coated copper dendrite electrocatalyst, the method comprising the following steps:

[0049] (1) Take a 1.5 cm 2 The foamed copper was immersed in 4M hydrochloric acid solution for 20 min to remove the surface oxide layer, washed with water and ethanol and then dried;

[0050] (2) placing the copper foam substrate in a 0.2 M copper sulfate solution, using a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and copper foam as a working electrode, electroplating at -1.1 V for 150 seconds, and washing with water to obtain copper dendrite-loaded copper foam;

[0051] (3) The copper dendrites were placed in a 0.15M nickel nitrate solution, with a saturated calomel electrode as the reference electrode, a carbon rod as the counter electrode, and a copper foam as the working electrode, and electrodeposited at -1.0V for 100 seconds, washed with water, and dried to obtain a nickel hydroxide-coated copper dendrite electrocatalyst. The SEM and TEM images of the nickel hydroxide-coated copper dendrite electrocatalyst obtained in Example 1 are shown in FIG. Figure 1The contact angle diagram of the nickel hydroxide-coated copper dendrite electrocatalyst obtained in Example 1 is shown in FIG. Figure 2 Specific Example 1 Raman map of copper dendrite electrocatalyst coated with nickel hydroxide Figure 3 The XRD pattern of the nickel hydroxide-coated copper dendrite electrocatalyst obtained in Example 1 is shown in Figure 4 The XPS graph of the copper dendrite electrocatalyst coated with nickel hydroxide obtained in Example 1 is shown in FIG. Figure 5 Specific Example 1 The linear sweep voltammetric curve of the copper dendrite electrocatalyst coated with nickel hydroxide is shown in FIG. Figure 6 Specific Example 1 Performance of Formaldehyde Oxidation and Hydrogen Production of Nickel Hydroxide-Coated Copper Dendrite Electrocatalyst Figure 7 Specific Example 1 The stability performance diagram of the copper dendrite electrocatalyst coated with nickel hydroxide is shown in Figure 8 Specific Example 1 Double layer capacitance curve of copper dendrite electrocatalyst coated with nickel hydroxide Fig. 9 .

[0052] First, the morphology and structure of the prepared nickel hydroxide-coated copper dendrite electrocatalyst were characterized by scanning and transmission electron microscopy, and it was found that the sample was a dendritic structure. From the transmission image, the dendritic morphology of the sample and the outer layer of nickel hydroxide were more clearly observed. The contact angle diagram proves that the catalyst surface is a hydrophilic surface after nickel hydroxide coverage. Through the Raman spectrum, nickel hydroxide and Cu-O bonds were observed, indicating the presence of nickel hydroxide. Through the XRD spectrum, only the peak of elemental copper was observed, and no obvious nickel hydroxide peak was observed, indicating that the nickel hydroxide was an amorphous structure. The XPS spectrum further confirmed the presence of nickel hydroxide. Next, the formaldehyde oxidation performance of copper dendrites coated with nickel hydroxide was investigated. In 1M potassium hydroxide and 0.25M formaldehyde electrolyte, a potential of only 0.1V is required to reach 400mA cm -2 The current density is 2.33 W, and the Faraday efficiency of hydrogen production by the catalyst at different potentials is close to 100%, indicating that the copper dendrite material coated with nickel hydroxide is an excellent catalyst for hydrogen production from formaldehyde oxidation. The cyclic stability of the copper dendrite coated with nickel hydroxide was tested. After 16 cycles, the catalyst performance was almost unchanged, indicating that it has excellent stability.

[0053] Embodiment 2:

[0054] A method for preparing a nickel hydroxide-coated copper dendrite electrocatalyst, the method comprising the following steps:

[0055] (1) Take a 1cm 2 The foamed copper was immersed in 1M hydrochloric acid solution for 5 min to remove the surface oxide layer, washed with water and ethanol and then dried;

[0056] (2) placing the copper foam substrate in a 0.1 M copper sulfate solution, using a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and copper foam as a working electrode, electroplating at -1.2 V for 100 seconds, and washing with water to obtain copper dendrite-loaded copper foam;

[0057] (3) The copper dendrites were placed in a 0.1 M nickel nitrate solution, with a saturated calomel electrode as the reference electrode, a carbon rod as the counter electrode, and copper foam as the working electrode. The solution was electrodeposited at -1.1 V for 50 seconds, washed with water, and dried to obtain a nickel hydroxide-coated copper dendrite electrocatalyst.

[0058] First, the morphology and structure of the prepared nickel hydroxide-coated copper dendrites were characterized by scanning, and it was found that the sample had a dendrite structure. Next, the formaldehyde oxidation performance of the nickel hydroxide-coated copper dendrites was explored. The test was carried out in 1M potassium hydroxide and 0.25M formaldehyde electrolyte, and it had excellent formaldehyde oxidation performance.

[0059] Embodiment 3:

[0060] A method for preparing a nickel hydroxide-coated copper dendrite electrocatalyst, the method comprising the following steps:

[0061] (1) Take a 4cm 2 The foamed copper was immersed in 6M hydrochloric acid solution for 30 min to remove the surface oxide layer, washed with water and ethanol and then dried;

[0062] (2) placing the copper foam substrate in a 0.3 M copper sulfate solution, using a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and copper foam as a working electrode, and electrodepositing at -1.0 V for 300 seconds, and washing with water to obtain copper dendrite-loaded copper foam;

[0063] (3) The copper dendrites were placed in a 0.2 M nickel nitrate solution, with a saturated calomel electrode as the reference electrode, a carbon rod as the counter electrode, and copper foam as the working electrode. The solution was electroplated at -0.9 V for 150 seconds, washed with water, and dried to obtain a nickel hydroxide-coated copper dendrite electrocatalyst.

[0064] First, the morphology and structure of the prepared nickel hydroxide-coated copper dendrites were characterized by scanning, and it was found that the sample had a dendrite structure. Next, the formaldehyde oxidation performance of the nickel hydroxide-coated copper dendrites was explored. The test was carried out in 1M potassium hydroxide and 0.25M formaldehyde electrolyte, and it had excellent formaldehyde oxidation performance.

[0065] Embodiment 4:

[0066] A method for preparing a nickel hydroxide-coated copper dendrite electrocatalyst, the method comprising the following steps:

[0067] (1) Take a 2cm 2The foamed copper was immersed in 4M hydrochloric acid solution for 20 min to remove the surface oxide layer, washed with water and ethanol and then dried;

[0068] (2) placing the copper foam substrate in a 0.2 M copper sulfate solution, using a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and copper foam as a working electrode, and electrodepositing at -1.1 V for 200 seconds, and washing with water to obtain copper dendrite-loaded copper foam;

[0069] (2) The copper dendrites were placed in a 0.15 M nickel nitrate solution, with a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and copper foam as a working electrode. The solution was electroplated at -1.0 V for 100 seconds, washed with water, and dried to obtain a nickel hydroxide-coated copper dendrite electrocatalyst.

[0070] First, the morphology and structure of the prepared nickel hydroxide-coated copper dendrites were characterized by scanning, and it was found that the sample had a dendrite structure. Next, the formaldehyde oxidation performance of the nickel hydroxide-coated copper dendrites was explored. The test was carried out in 1M potassium hydroxide and 0.25M formaldehyde electrolyte, and it had excellent formaldehyde oxidation performance.

Claims

1. A nickel hydroxide-coated copper dendrite electrocatalyst, characterized in that: Prepared by the following method: (1) Take a piece of 1-4 cm 2 The foamed copper was immersed in a 1-6M hydrochloric acid solution for 5-30 minutes to remove the surface oxide layer, washed with water and ethanol and then dried; (2) placing the copper foam substrate in a 0.1-0.3M copper sulfate solution, using a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and copper foam as a working electrode, electroplating for 100-300 seconds at -1.2--1.0V, and washing with water to obtain copper dendrite-loaded copper foam; (3) The copper dendrites are placed in a 0.1-0.2M nickel nitrate solution, with a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and a copper foam as a working electrode. The copper dendrites are electrodeposited at -1.1 to -0.9V for 50 to 150 seconds, washed with water, and dried to obtain a nickel hydroxide-coated copper dendrite electrocatalyst.

2. A method for preparing the nickel hydroxide-coated copper dendrite electrocatalyst as claimed in claim 1, characterized in that: The method comprises the following steps: (1) Take a piece of 1-4 cm 2 The foamed copper was immersed in a 1-6M hydrochloric acid solution for 5-30 minutes to remove the surface oxide layer, washed with water and ethanol and then dried; (2) placing the copper foam substrate in a 0.1-0.3M copper sulfate solution, using a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and copper foam as a working electrode, electroplating for 100-300 seconds at -1.2--1.0V, and washing with water to obtain copper dendrite-loaded copper foam; (3) The copper dendrites are placed in a 0.1-0.2M nickel nitrate solution, with a saturated calomel electrode as a reference electrode, a carbon rod as a counter electrode, and a copper foam as a working electrode. The copper dendrites are electrodeposited at -0.1 to -0.9V for 50 to 150 seconds, washed with water, and dried to obtain a nickel hydroxide-coated copper dendrite electrocatalyst.

3. The method for preparing the nickel hydroxide-coated copper dendrite electrocatalyst according to claim 2, characterized in that: The morphology and structure of the material can be controlled by adjusting the concentration of copper sulfate and nickel nitrate, the potential and time of electrodeposition.

4. The method for preparing the nickel hydroxide-coated copper dendrite electrocatalyst according to claim 2 or 3, characterized in that: The thickness of the nickel hydroxide is 5-7 nm.

Citation Information

Patent Citations

  • Method for producing hydrogen through selective oxidation coupling of alcohol or aldehyde

    CN113774398A

  • Method for preparing polycarboxylic acid by electrocatalytic oxidation of aldehydes and alcohols

    CN114574881A

  • System and methods for low-voltage bipolar hydrogen production from aldehydes and water

    US20230332307A1