Preparation method of carbon-supported platinum group catalyst

By using biomass materials to prepare nitrogen-containing carbon support and combining complex encapsulation technology of platinum group metal ions and organic copolymers, the problems of uneven particle size and reduction competition in carbon-supported platinum group catalysts are solved, and platinum group metals are realized The uniform distribution of particles and high catalytic activity are suitable for large-scale production.

CN118996514APending Publication Date: 2024-11-22HUAYI NEW ENERGY MATERIALS (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411041155.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The carbon support particles of existing carbon-supported platinum group catalysts are uneven in size, and there are problems such as competition for metal ion reduction and insufficient reaction, which limits its application in the new energy industry.

Method used

The nitrogen-containing carbon carrier is prepared by using biomass materials, and the carbon carriers are wrapped by high-pressure liquid phase reaction and acid irradiation treatment, combining the complex of platinum group metal ions and organic copolymers to limit the reduction of platinum group metal ions on the surface of carbon carriers and avoid reducing competition. , a uniform distribution of platinum group metal particles is formed.

Benefits of technology

The uniform distribution of platinum group metal particles in carbon-supported platinum group catalysts is achieved, which improves catalytic activity, is suitable for large-scale production, and reduces equipment and process costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996514A_ABST
    Figure CN118996514A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a carbon-supported platinum group catalyst, the preparation method adopts a biomass material as a raw material for preparing a nitrogen-containing carbon carrier, and the adopted platinum group metal source exists in the form of a complex of platinum group metal ions and an organic copolymer. The carbon-supported platinum group catalyst obtained by the preparation method has uniform distribution of platinum group metal particles, the nitrogen-carbon ratio of the carrier material is flexible and adjustable, the problems of reduction competition and insufficient reaction of metal ions when two or more platinum group metals are subjected to liquid-phase reduction at the same time are solved, the particle size distribution of the carrier is uniform, and the catalyst has a good application prospect. The catalyst prepared by the method can provide a higher specific surface area for a catalytic material, has more effective catalytic active sites, and is more stable in catalytic reaction compared with an existing commercial catalyst. The preparation method has the advantages of low price of required equipment, simple preparation process, no need of fine regulation and control on details, and suitableness for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon materials, and in particular relates to a method for preparing a carbon-supported platinum group catalyst. Background Art

[0002] Currently, the best performing and most widely used commercial water electrolysis hydrogen production catalyst is the carbon-supported platinum group catalyst.

[0003] Carbon-supported platinum group catalysts include carbon carriers and platinum group nanoparticles supported on the carbon carriers. Currently, commercial carbon carriers with a high market share are mostly obtained by pyrolysis and carbonization of small molecules such as oleic acid, linolenic acid, naphtha and acetylene. Due to the existence of foreign patents and technical barriers, there are risks to the development of my country's new energy industry, and the carbon carriers obtained by pyrolysis and carbonization of these small molecules have the problem of uneven particle size.

[0004] In addition, research on low-platinum catalysts has shown that the mass activity of platinum can be further improved by constructing bimetallic or multimetallic alloy sites of platinum group metals to replace traditional elemental platinum nanoparticle sites and utilizing the synergistic effect of bimetallic or multimetallic alloy sites. However, these bimetallic or multimetallic alloy schemes of the platinum group are difficult to scale up for industrialization due to the reduction competition between metal ions and differences in reduction efficiency. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing a carbon-supported platinum group catalyst. The carbon carrier particles obtained by the preparation method have uniform sizes, so as to overcome the shortcomings of the prior art.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A method for preparing a carbon-supported platinum group catalyst comprises the following steps:

[0008] (1) soaking the crushed and broken biomass material in an organic solvent, and then filtering and rotary evaporating to remove part of the organic solvent to form an organic dispersion;

[0009] (2) subjecting the organic dispersion to a high-pressure liquid phase reaction, and after the reaction is completed, rotary evaporation is performed to remove all organic solvents to obtain an asphalt-like product;

[0010] (3) subjecting the asphalt-like product to a thorough acid leaching treatment, and after the acid leaching, immersing the solid product in a weakly alkaline aqueous solution to adjust the pH to neutral, and finally drying to obtain a nitrogen-containing carbon carrier;

[0011] (4) dispersing the nitrogen-containing carbon support in a platinum group metal source solution to form a stable dispersion;

[0012] (5) adjusting the pH value of the stable dispersion to 11-14, adding a sodium borohydride aqueous solution, and after the reaction, centrifuging, washing, and drying the reaction product to obtain a black powder;

[0013] (6) The black powder is calcined under the protection of an inert gas at a temperature of 350-800° C. After calcination, the powder is cooled to room temperature to obtain a carbon-supported platinum group catalyst.

[0014] By adopting the above technical scheme, biomass materials (i.e. dried leaves) are used as raw materials for preparing nitrogen-containing carbon carriers, and the carbon carrier particles prepared by high-pressure liquid phase reaction are uniform in size, with the size distribution of the carbon carrier being around 40 nanometers, and the size distribution of the platinum group metal particles being 2-3 nanometers. In addition, the preparation does not require expensive equipment, the process is simple, and it is suitable for production scale-up.

[0015] In the present invention, the platinum group metal source comprises one, two or more platinum group elements, that is, the present invention can construct a bimetallic or multimetallic alloy site of platinum group metals.

[0016] In the present invention, the platinum group metal source exists in the form of a complex of platinum group metal ions and an organic copolymer. In the present invention, the platinum group metal source exists in the form of a complex of platinum group metal ions and an organic copolymer, and the complex is wrapped on the surface of the nitrogen-containing carbon carrier of the present invention through stirring and adsorption, and the platinum group noble metal cations are confined to the surface of the carbon carrier through complexation. Due to the spatial confinement effect of the polymer molecules, one or more platinum group metal ions are reduced nearby on the surface of the carbon carrier, and the loss of ions and uneven alloy catalytic sites caused by reduction competition are prevented, which can improve the reaction efficiency of metal ions, make the reduction reaction more sufficient, and increase the content of platinum group metals in the prepared carbon-supported platinum group catalyst.

[0017] In the present invention, the platinum group metal ions are derived from salts or hydrates of platinum group elements, such as dichlorides, trichlorides, tetrachlorides, nitrates or hydrochloric acid tetrachloride hydrates of platinum group elements.

[0018] The organic polymer is maleic acid, vinyl alcohol, polyacrylic acid, soluble chitosan or starch.

[0019] The method for forming the complex is as follows: dripping an aqueous solution containing platinum group metal ions into an aqueous solution of an organic polymer, maintaining an ice water bath and stirring during the dripping process, and operating in the dark throughout the process. The molar ratio of the organic copolymer dissolved in the aqueous solution is calculated as monomer, the molar ratio of the amount of polymer monomer substance to the amount of water molecules is 0.01-5%, and the molar ratio of the amount of platinum group metal salt to the amount of the organic copolymer, calculated as monomer, is (0.01-5):1.

[0020] In the present invention, in order to prepare a nitrogen-containing carbon carrier with a high nitrogen content, melamine, ammonium cyanide, ammonium carbonate, ammonium nitrate or polyvinyl pyrrolidone is added in the high-pressure liquid phase reaction. The nitrogen content can be adjusted by adding nitrogen-containing substances in the high-pressure liquid phase.

[0021] In the present invention, the high-pressure liquid phase reaction is to place the filtered organic dispersion in an autoclave for heating at a temperature of 180-360° C. for 2-8 hours, and then cool down naturally.

[0022] In the present invention, the organic solvent is methanol, ethanol, propanol, butanol, sec-butanol, ethylene glycol, cyclohexane, ethyl acetate or butanone.

[0023] In the present invention, the acid used in the acid shower is oxalic acid, hydrochloric acid, acetic acid or nitric acid.

[0024] The carbon-supported platinum group catalyst obtained by the preparation method of the present invention has a uniform distribution of platinum group metal particles, wherein the particle size of the nitrogen-containing carbon carrier is about 40 nanometers, and the size distribution of the platinum group metal nanoparticles loaded thereon is around 2.6 nanometers, wherein the nitrogen-carbon ratio of the carrier material is flexibly adjustable, and the nitrogen content is distributed in the range of 5-10%, and the problems of reduction competition of metal ions and insufficient reaction existing when two or more platinum group metals are simultaneously reduced in liquid phase are solved, and the particle size distribution of the carrier is uniform, which can provide a higher specific surface area for the catalytic material and has more effective catalytic active sites. In addition, the equipment required for this method is low-priced, has a simple preparation process, does not require fine regulation of each detail, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1A Transmission electron microscope (TEM) image of nitrogen-containing carbon support prepared by excessive addition of melamine;

[0026] Figure 1B Transmission electron microscope (TEM) image of nitrogen-containing carbon support prepared by excessive addition of polyvinyl pyrrolidone;

[0027] Figure 2 This is a transmission electron microscope (TEM) image of the carbon-supported platinum group catalyst prepared in Example 4;

[0028] Figure 3 This is a particle size distribution diagram of carbon nanoparticles of the carbon-supported platinum group catalyst prepared in Example 4;

[0029] Figure 4 is a particle size distribution diagram of platinum nanoparticles of the carbon-supported platinum group catalyst prepared in Example 4;

[0030] Figure 5 This is the XPS spectrum of the carbon-supported platinum group catalyst prepared in Example 4;

[0031] Figure 6 This is a comparison chart of the LSV of the carbon-supported platinum group catalyst prepared in Example 4 and the commercial platinum-carbon catalyst at the water electrolysis hydrogen production end.

[0032] Figure 7 The voltage change curves of the carbon-supported platinum group catalyst prepared in Example 4 and the commercial platinum-carbon catalyst during the constant current test at the hydrogen production end. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below with reference to the embodiments.

[0034] Example 1

[0035] (1) The dried leaves are crushed and soaked in methanol for 24 hours to obtain a yellow-green solution, and filtered through an organic filter membrane with a pore size of 0.22 μm to obtain a yellow-green organic solution free of particulate impurities. The organic solvent is removed by moderate rotary evaporation to obtain a coffee-colored organic dispersion with a laundry detergent viscosity;

[0036] (2) placing the organic dispersion in an autoclave for reaction at a temperature of 180° C. for a reaction time of 4 hours, cooling naturally, and after the reaction is completed, removing all organic solvents by rotary evaporation to obtain an asphalt-like product;

[0037] (3) The asphalt-like reactant is fully treated with acetic acid leaching. After the acid leaching, the solid product is immersed in a sodium bicarbonate (NaHCO3) aqueous solution, filtered and washed with pure water at least three times, and finally dried to obtain a nitrogen-containing carbon carrier.

[0038] Example 2

[0039] (1) The dried leaves are crushed and soaked in sec-butyl alcohol for 24 hours to obtain a yellow-green solution, and filtered through an organic filter membrane with a pore size of 0.22 μm to obtain a yellow-green organic solution free of particulate impurities. The organic solvent is removed by appropriate rotary evaporation to obtain a coffee-colored organic dispersion with a laundry detergent viscosity;

[0040] (2) placing the organic dispersion in an autoclave, adding melamine powder, the mass ratio of melamine to organic dispersion being 1%, the reaction temperature being 300° C., the reaction time being 4 hours, and cooling naturally. After the reaction is completed, removing all organic solvents by rotary evaporation to obtain an asphalt-like product;

[0041] (3) The asphalt-like product is fully treated with oxalic acid. After the acid leaching, the solid product is immersed in a sodium bicarbonate (NaHCO3) aqueous solution, and finally dried to obtain a nitrogen-containing carbon carrier.

[0042] <Determination of Nitrogen Content of Carbon Support>

[0043] The nitrogen-containing carbon supports prepared in Example 1 and Example 2 were respectively subjected to X-ray photoelectron spectroscopy (XPS) analysis and determination, and the test data are shown in Table 1.

[0044] Table 1

[0045]

[0046] As can be seen from Table 1, the nitrogen element in the carbon carrier mainly comes from the molecules in the organic solution after the biomass before the high-pressure liquid phase reaction is extracted with an organic solvent, mainly various types of chlorophyll molecules. Through testing, the average mass content of nitrogen in the nitrogen-containing carbon carrier obtained in Example 1 reached 6.4%. In Example 2, by adding melamine, an organic small molecule with a high nitrogen content, the nitrogen content in the carbon carrier can be increased during the high-pressure liquid phase reaction. After testing, the average mass content of nitrogen in the nitrogen-containing carbon carrier obtained in Example 2 reached 8.2%. This shows that by adding small organic molecules, polymer molecules, nitrates, ammonium salts, cyanide salts and other methods with a high nitrogen content, the nitrogen content in the nitrogen-containing carbon carrier can be increased in a high-pressure liquid phase reaction.

[0047] However, the regulation of nitrogen is not unlimited. Taking the addition of melamine as an example, when the mass ratio of the added melamine to the mass ratio of the organic dispersion obtained in step (1) of Example 2 exceeds 1%, the effect of the high-pressure liquid phase reaction becomes worse, resulting in that it is more difficult to form carbon nanoparticles and more likely to form amorphous carbon nanoflowers and other flaky nanostructures.

[0048] After replacing melamine with polyvinyl pyrrolidone or ammonium nitrate salt, a similar phenomenon of the dosage mass affecting the formation of nanoparticles occurred. The difference lies in the ratio of the nitrogen-doped regulated molecular dosage mass to the mass of the organic dispersion.

[0049] For example, in other embodiments of preparing nitrogen-containing carbon carriers, the same reaction conditions as in Example 2 were used, but an excess of melamine (the mass ratio of the added mass to the organic dispersion was 2%) or an excess of polyvinyl pyrrolidone (the mass ratio of the added mass to the organic dispersion was 4%) was added, and the obtained nitrogen-containing carbon carriers were photographed by transmission electron microscopy (TEM), respectively, and the following were obtained: Figure 1A and Figure 1B The image shown. Figure 1A or Figure 1B It can be seen that excessive addition of melamine and excessive addition of polyvinyl pyrrolidone will form amorphous carbon nanoflowers but cannot form carbon nanoparticles.

[0050] Therefore, in the present invention, if the nitrogen content of the carbon carrier needs to be adjusted, the amount of nitrogen-containing substance added in the organic dispersion is uniformly not higher than 1% of the mass of the organic dispersion to prevent the generation of amorphous nanostructures.

[0051] Example 3

[0052] (1) 34.8 mg of polymaleic acid was dispersed in 10 ml of deionized water, and 310 mg of chloroplatinic acid (H2PtCl6·6H2O) was added to the polymaleic acid dispersion. The dispersion process was maintained in an ice-water bath environment. The reaction conditions were to avoid light, stir slowly, and allow to react overnight.

[0053] (2) 100 mg of the nitrogen-containing carbon support prepared in Example 1 was ultrasonically dispersed in a mixed solution of chloroplatinic acid and polymaleic acid. After uniform dispersion, the pH value of the mixed solution was adjusted to 11 using 2 mol / L sodium hydroxide (NaOH), and stirring was continued for 12 hours. The reaction was kept away from light.

[0054] (3) Take 20 ml of a sodium borohydride (NaBH4) aqueous solution with a molar concentration of 0.2 mol / L and add it dropwise into the mixed solution. Continue the reaction for 4 hours until it ends.

[0055] (4) After the reaction is completed, a black powder solid is obtained by centrifugation, washing with water and drying.

[0056] (5) The obtained black powder solid is calcined under nitrogen protection at a calcination temperature of 600° C., kept at 600° C. for 1 hour, and naturally cooled to room temperature to obtain a black powder.

[0057] Example 4

[0058] (1) 34.8 mg of polymaleic acid was dispersed in 10 ml of deionized water, and then 155 mg of chloroplatinic acid (H2PtCl6·6H2O) was added to the polymaleic acid dispersion. The dispersion process was kept in an ice-water bath environment. The reaction conditions were to avoid light, stir slowly, and leave overnight.

[0059] (2) 100 mg of the nitrogen-containing carbon support prepared in Example 1 was ultrasonically dispersed in a mixed solution of chloroplatinic acid and polymaleic acid. After uniform dispersion, the pH value of the mixed solution was adjusted to 11 using 2 mol / L sodium hydroxide (NaOH), and stirring was continued for 12 hours. The reaction was kept away from light.

[0060] (3) Take 10 ml of a sodium borohydride (NaBH4) aqueous solution with a molar concentration of 0.2 mol / L and add it dropwise into the mixed solution. Continue the reaction for 4 hours until it ends.

[0061] (4) After the reaction is completed, a black powder solid is obtained by centrifugation, washing with water and drying.

[0062] (5) The obtained black powder solid is calcined under nitrogen protection at a calcination temperature of 600° C., kept at 600° C. for 1 hour, and naturally cooled to room temperature to obtain a black powder.

[0063] Example 5

[0064] (1) Disperse 52.2 mg of polymaleic acid in 10 ml of deionized water, take 155 mg of chloroplatinic acid (H2PtCl6·6H2O) and 68 mg of rhodium chloride (RhCl3·3H2O) and add them to the polymaleic acid dispersion. Keep the dispersion in an ice-water bath environment. The reaction conditions are to avoid light, stir slowly, and keep overnight.

[0065] (2) 100 mg of the nitrogen-containing carbon support prepared in Example 1 was ultrasonically dispersed in a mixed solution of chloroplatinic acid, rhodium chloride and polymaleic acid. After uniform dispersion, the pH value of the mixed solution was adjusted to 14 using 2 mol / L sodium hydroxide (NaOH), and stirring was continued for 12 hours. The reaction was kept away from light.

[0066] (3) Take 20 ml of a sodium borohydride (NaBH4) aqueous solution with a molar concentration of 0.2 mol / L and add it dropwise into the mixed solution. Continue the reaction for 4 hours until it ends.

[0067] (4) After the reaction is completed, a black powder solid is obtained by centrifugation, washing with water and drying.

[0068] (5) The obtained black powder solid is calcined under nitrogen protection at a calcination temperature of 800° C., kept at 800° C. for 1 hour, and naturally cooled to room temperature to obtain a black powder.

[0069] Example 6

[0070] (1) Disperse 26.4 ml of polyvinyl alcohol in 10 ml of deionized water, take 155 mg of chloroiridic acid (H2IrCl6·6H2O) and add it to the polyvinyl alcohol dispersion. Keep the dispersion in an ice-water bath. The reaction conditions are to avoid light, stir slowly, and keep overnight.

[0071] (2) 100 mg of the nitrogen-containing carbon support prepared in Example 1 was ultrasonically dispersed in a mixed solution of chloroiridic acid and polyvinyl alcohol. After uniform dispersion, the pH value of the mixed solution was adjusted to 13 using 2 mol / L sodium hydroxide (NaOH), and stirring was continued for 12 hours. The reaction was kept away from light.

[0072] (3) Take 10 ml of a sodium borohydride (NaBH4) aqueous solution with a molar concentration of 0.2 mol / L and add it dropwise into the mixed solution. Continue the reaction for 4 hours until it ends.

[0073] (4) After the reaction is completed, a black powder solid is obtained by centrifugation, washing with water and drying.

[0074] (5) The obtained black powder solid is calcined under nitrogen protection at a calcination temperature of 450° C., kept at 450° C. for 1 hour, and naturally cooled to room temperature to obtain a black powder.

[0075] Example 7

[0076] (1) Disperse 52.8 mg of polyvinyl alcohol in 10 ml of deionized water, take 155 mg of chloroiridic acid (H2PtCl6·6H2O) and 78 mg of ruthenium chloride (RuCl3·3H2O) and add them to the polyvinyl alcohol dispersion. Keep the dispersion in an ice-water bath environment. The reaction conditions are to avoid light, stir slowly, and keep overnight.

[0077] (2) 100 mg of the nitrogen-containing carbon support prepared in Example 1 was ultrasonically dispersed in a mixed solution of chloroiridic acid, ruthenium chloride and polyvinyl alcohol. After uniform dispersion, the pH value of the mixed solution was adjusted to 13 using 2 mol / L sodium hydroxide (NaOH), and stirring was continued for 12 hours. The reaction was kept away from light.

[0078] (3) Take 20 ml of a sodium borohydride (NaBH4) aqueous solution with a molar concentration of 0.2 mol / L and add it dropwise to the mixed solution. Continue the reaction for 4 hours until it ends.

[0079] (4) After the reaction is completed, a black powder solid is obtained by centrifugation, washing with water and drying.

[0080] (5) The obtained black powder solid is calcined under nitrogen protection at a calcination temperature of 700° C., kept at 700° C. for 1 hour, and naturally cooled to room temperature to obtain a black powder.

[0081] Example 8

[0082] (1) Disperse 21.6 mg of polyacrylic acid in 10 ml of deionized water, take 127.8 mg of palladium chloride (PdCl2·2H2O) and add it to the polyacrylic acid dispersion. Keep the dispersion in an ice-water bath environment. The reaction conditions are to avoid light, stir slowly, and keep overnight.

[0083] (2) 100 mg of the nitrogen-containing carbon support prepared in Example 1 was ultrasonically dispersed in a mixed solution of palladium chloride and polyacrylic acid. After uniform dispersion, 2 mol / L sodium hydroxide (NaOH) was used to adjust the pH value of the mixed solution to 13, and stirring was continued for 12 hours. The reaction was kept away from light.

[0084] (3) Take 20 ml of a sodium borohydride (NaBH4) aqueous solution with a molar concentration of 0.2 mol / L and add it dropwise into the mixed solution. Continue the reaction for 4 hours until it ends.

[0085] (4) After the reaction is completed, a black powder solid is obtained by centrifugation, washing with water and drying.

[0086] (5) The obtained black powder solid is calcined under nitrogen protection at a calcination temperature of 600° C., kept at 600° C. for 1 hour, and naturally cooled to room temperature to obtain a black powder.

[0087] Comparative Example 1

[0088] (1) Take 155 mg of chloroplatinic acid (H2PtCl6·6H2O) and 68 mg of rhodium chloride (RhCl3·3H2O) and disperse them in 10 ml of deionized water. Keep the dispersion environment in an ice water bath. The reaction conditions are to avoid light, stir slowly, and keep overnight.

[0089] (2) 100 mg of the nitrogen-containing carbon support prepared in Example 1 was ultrasonically dispersed in the above dispersion. After uniform dispersion, 2 mol / L sodium hydroxide (NaOH) was used to adjust the pH value of the mixed solution to 14, and stirring was continued for 12 hours. The reaction was kept away from light.

[0090] (3) Take 20 ml of a sodium borohydride (NaBH4) aqueous solution with a molar concentration of 0.2 mol / L and add it dropwise into the mixed solution. Continue the reaction for 4 hours until it ends.

[0091] (4) After the reaction is completed, a black powder solid is obtained by centrifugation, washing with water and drying.

[0092] (5) The obtained black powder solid is calcined under nitrogen protection at a calcination temperature of 800° C., kept at 800° C. for 1 hour, and naturally cooled to room temperature to obtain a black powder.

[0093] Comparative Example 2

[0094] (1) 194 mg of chloroplatinic acid (H2PtCl6·6H2O) and 87.9 mg of rhodium chloride (RhCl3·3H2O) were dispersed in 10 ml of deionized water. The dispersion process was kept in an ice-water bath environment. The reaction conditions were to avoid light, stir slowly, and leave overnight.

[0095] (2) 100 mg of nitrogen-doped carbon was ultrasonically dispersed in the above dispersion. After uniform dispersion, the pH value of the mixed solution was adjusted to 14 using 2 mol / L sodium hydroxide (NaOH), and stirring was continued for 12 hours. The reaction was protected from light throughout the process.

[0096] (3) Take 20 ml of a sodium borohydride (NaBH4) aqueous solution with a molar concentration of 0.2 mol / L and add it dropwise into the mixed solution. Continue the reaction for 4 hours until it ends.

[0097] (4) After the reaction is completed, a black powder solid is obtained by centrifugation, water washing and drying. (5) The obtained black powder solid is calcined under nitrogen protection at a calcination temperature of 800° C., kept at 800° C. for 1 hour, and naturally cooled to room temperature to obtain a black powder.

[0098] <Testing of platinum group metal content in Examples 3 to 8>

[0099] The platinum group metal contents of the carbon-supported platinum group catalysts prepared in Examples 3 to 8 were measured using inductively coupled plasma mass spectrometry (IPC-MS) technology, and the platinum group metal contents were shown in Table 2.

[0100] Table 2

[0101]

[0102] From Table 2 above, it can be seen that the carbon-supported platinum group catalyst prepared in each example was randomly tested 5 times. According to the average content of platinum group metals in the carbon-supported platinum group catalyst prepared in each example, it can be known that:

[0103] The carbon-supported platinum group catalyst prepared in Example 3 has 10% by mass of metal platinum loaded on the carbon support;

[0104] The carbon-supported platinum group catalyst prepared in Example 4 has 5% by mass of metal platinum loaded on the carbon support;

[0105] The carbon-supported platinum group catalyst prepared in Example 5 is loaded with 5% by mass of metal platinum and 5% by mass of metal rhodium on the carbon support;

[0106] The carbon-supported platinum group catalyst prepared in Example 6 has iridium metal loaded on the carbon support in an amount of 5% by mass;

[0107] The carbon-supported platinum group catalyst prepared in Example 7 is loaded with 5% by mass of metallic iridium and 5% by mass of metallic ruthenium on the carbon support;

[0108] The carbon-supported platinum group catalyst prepared in Example 8 is loaded with 10% by mass of metallic palladium on the carbon support.

[0109] <Test of platinum group metal content in Comparative Example 1 and Comparative Example 2>

[0110] The platinum group metal contents of the carbon-supported platinum group catalysts prepared in Comparative Example 1 and Comparative Example 2 were measured using inductively coupled plasma mass spectrometry (IPC-MS) technology, and the platinum group metal contents were shown in Table 3.

[0111] Table 3

[0112]

[0113] Comparative Examples 1 and 2 are compared with Example 5. In Comparative Example 1, compared with Example 5, the amount of platinum group metal salt used is not changed, but the aqueous solution of the metal salt is directly blended with the nitrogen-containing carbon carrier, and the reaction conditions are consistent with those of Example 5. The obtained metal contents are all low, as shown in Table 3, wherein the mass content of platinum (Pt) is 3.70%, and the mass content of rhodium (Rh) is 3.79%, which are lower than the mass content of platinum (Pt) (5.14%) and the mass content of rhodium (Rh) (5.06%) in Example 5.

[0114] In Comparative Example 2, the aqueous solution of the metal salt and the nitrogen-containing carbon carrier are still blended as the method of adding the platinum group metal salt, but the amount of the platinum group metal salt used is increased. In Comparative Example 2, the amount of chloroplatinic acid used is increased by 25%, from 155 mg to 194 mg, and the amount of rhodium trichloride used is increased by 30%, from 68 mg to 87.9 mg. Under the same reaction conditions as in Example 5, the metal percentage reaches a value close to that in Example 5, the mass content of platinum (Pt) is 5.14%, and the mass content of rhodium (Rh) is 4.97%, both of which are close to the mass content of platinum (Pt) (5.14%) and the mass content of rhodium (Rh) (5.06%) in Example 5.

[0115] The above two control experiments respectively verified that using a complex of polymer macromolecules and metal salts as a method of adding platinum group metal salts can improve the reaction utilization efficiency of metal ions.

[0116] <Testing of the Carbon-Supported Platinum Group Catalyst Prepared in Example 4>

[0117] Figure 2 This is a transmission electron microscope image of the carbon-supported platinum group catalyst prepared in Example 4. The agglomerated particles are spherical nitrogen-containing carbon carriers, and the darker small particles inside are nano-metal platinum.

[0118] Figure 3 This is a statistical diagram of the carbon nanometer size distribution in the carbon-supported platinum group catalyst prepared in Example 4. From this figure, it can be seen that the center size of the nitrogen-containing carbon carrier is about 40 nanometers.

[0119] Figure 4 This is a statistical diagram of the size distribution of platinum nanoparticles in the carbon-supported platinum group catalyst prepared in Example 4. From this figure, it can be seen that the center size of the metal platinum particles is about 2.68 nanometers.

[0120] Figure 5This is the XPS spectrum of the carbon-supported platinum group catalyst prepared in Example 4. XPS (X-ray photoelectron spectroscopy) analysis shows that the obtained catalyst mainly contains carbon, nitrogen, and platinum metal elements. The nitrogen content is about 7%, and the platinum peak is at 70 electron volts, which is clear and obvious, indicating that the aggregation degree of platinum elements is relatively high, which is consistent with the situation of platinum nanoparticles seen by transmission electron microscopy.

[0121] Figure 6 The linear sweep voltammetric curves of the carbon-supported platinum catalyst prepared in Example 4 and the commercial platinum-carbon catalyst (Johnson Matthey Hispec 4000 platinum-carbon catalyst, platinum content 40%) were measured in an argon-saturated 0.5M H2SO4 solution (pH = 0). The comparative current density is 10 mA / cm 2 The overpotential of the carbon-supported platinum catalyst prepared in Example 4 is 52.6 mV, which is lower than the overpotential (57.1 mV) of the commercial catalyst with a platinum loading of 40% by mass. This shows that the carbon-supported platinum catalyst prepared in Example 4 has a lower platinum loading than the commercial catalyst with a higher platinum loading, and has obvious advantages in hydrogen production by electrolysis of water, and has strong substitutability.

[0122] Figure 7 The constant current method long cycle voltage stability test data of the carbon-supported platinum catalyst prepared in Example 4 and the commercial platinum-carbon catalyst (Johnson Matthey Hispec 4000 platinum-carbon catalyst, platinum content 40%) for decomposing water to produce hydrogen in an argon-saturated 0.5M H2SO4 solution (pH=0) are given. It can be seen from the data in the figure that after 40 hours of constant current testing, the voltage change of the carbon-supported platinum catalyst in Example 4 is no more than 3mV, which is lower than the 8mV voltage change of the commercial platinum-carbon catalyst, indicating that the carbon-supported platinum catalyst prepared in Example 4 has a more stable catalytic performance.

Claims

1. A method for preparing a carbon-supported platinum group catalyst, characterized in that: The steps include: (1) soaking the crushed and broken biomass material in an organic solvent, and then filtering and rotary evaporating to remove part of the organic solvent to form an organic dispersion; (2) subjecting the organic dispersion to a high-pressure liquid phase reaction, and after the reaction is completed, rotary evaporation is performed to remove all organic solvents to obtain an asphalt-like product; (3) subjecting the asphalt-like product to a thorough acid leaching treatment, and after the acid leaching, immersing the solid product in a weakly alkaline aqueous solution to adjust the pH to neutral, and finally drying to obtain a nitrogen-containing carbon carrier; (4) dispersing the nitrogen-containing carbon support in a platinum group metal source solution to form a stable dispersion; (5) adjusting the pH value of the stable dispersion to 11-14, adding an aqueous solution of sodium borohydride, and after the reaction, centrifuging, washing, and drying the reaction product to obtain a black powder; (6) The black powder is calcined under the protection of an inert gas at a temperature of 350-800° C. After calcination, the powder is cooled to room temperature to obtain a carbon-supported platinum group catalyst.

2. The method for preparing a carbon-supported platinum group catalyst according to claim 1, characterized in that: The platinum group metal source comprises one, two or more platinum group elements.

3. The method for preparing a carbon-supported platinum group catalyst according to claim 2, characterized in that: The platinum group metal source exists in the form of a complex of platinum group metal ions and an organic copolymer.

4. The method for preparing a carbon-supported platinum group catalyst according to claim 3, characterized in that: The platinum group metal ions are derived from salts or salt hydrates of platinum group elements.

5. The method for preparing a carbon-supported platinum group catalyst according to claim 3, characterized in that: The organic polymer is maleic acid, vinyl alcohol, polyacrylic acid, soluble chitosan or starch.

6. The method for preparing a carbon-supported platinum group catalyst according to claim 3, characterized in that: The aqueous solution containing platinum group metal ions is added dropwise to the aqueous solution of the organic polymer. During the dropping process, an ice water bath is maintained and stirring is performed. The whole process is performed in a dark environment.

7. The method for preparing a carbon-supported platinum group catalyst according to claim 1, characterized in that: Melamine, ammonium cyanide, ammonium carbonate, ammonium nitrate or polyvinyl pyrrolidone is added during the high pressure liquid phase reaction.

8. The method for preparing a carbon-supported platinum group catalyst according to claim 1, characterized in that: The high-pressure liquid phase reaction is to place the filtered organic dispersion in an autoclave and heat it at a temperature of 180-360° C. for 2-8 hours, and then cool it down naturally.

9. The method for preparing a carbon-supported platinum group catalyst according to claim 1, characterized in that: The organic solvent is methanol, ethanol, propanol, butanol, sec-butanol, ethylene glycol, cyclohexane, ethyl acetate or butanone.

10. The method for preparing a carbon-supported platinum group catalyst according to claim 1, characterized in that: The acid used in the acid leaching is oxalic acid, hydrochloric acid, acetic acid or nitric acid.