Impregnating emulsion for scratch-resistant formaldehyde-free impregnated decorative paper and preparation method of impregnating emulsion
By introducing nano-apatite and organosilicon-modified polyurethane-acrylate resin into impregnated decorative paper, the problem of insufficient scratch resistance of formaldehyde-free impregnated decorative paper was solved, achieving formaldehyde-free status and improved surface hardness.
Patent Information
- Application Number
- CN202411375218.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing formaldehyde-free impregnated decorative paper is prone to surface scratches during the pressing process, affecting surface quality and having insufficient scratch resistance.
Nano-apatite is used as a filler dispersed in the resin, combined with silicone-modified polyurethane-acrylate resin, to improve the surface hardness of the impregnated decorative paper and enhance its scratch resistance.
The surface hardness of the formaldehyde-free impregnated decorative paper has been improved, and its scratch resistance has been significantly enhanced, meeting the relevant standard requirements.
Smart Images

Figure CN118996908A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material processing, in particular to an impregnation emulsion for scratch-resistant formaldehyde-free impregnated decorative paper and a preparation method thereof. Background Art
[0002] Impregnated decorative paper is made of decorative base paper after printing and impregnation with resin. It is widely used in the surface decoration of artificial boards, accounting for about 65% of the market for surface decoration materials. It can not only beautify and decorate artificial boards, but also give them excellent surface properties including pollution resistance, water vapor resistance, scratch resistance, etc. For a long time, impregnation resins have mostly used urea-formaldehyde resins or melamine-formaldehyde resins. This type of resin releases formaldehyde during production and use, which is harmful to workers and consumers. With the improvement of people's environmental awareness and the introduction of relevant national laws and regulations. The production of formaldehyde-free veneer artificial board products is an important direction for future development. At present, artificial board products prepared with soy protein glue, lignin glue or isocyanate glue have been prepared. The Wood Industry Research Institute of the Chinese Academy of Forestry (ZL202010394895.7), the New Forestry Technology Research Institute of the Chinese Academy of Forestry (ZL202010394935.8), and Guangdong Tianyuan Huibang New Materials Co., Ltd. (ZL201811302724.6) have developed polyurethane / polyacrylate resins with low polymerization degree, high permeability, and high solid content. They use monomers with active groups such as hydroxyl / amine groups and modified additives to construct impregnation resin systems for formaldehyde-free impregnated film paper with different functions, and produce formaldehyde-free impregnated decorative paper products, which have good finishing effects on different artificial board substrates. However, this type of formaldehyde-free impregnated decorative paper products has insufficient surface scratch resistance, and the surface is easily scratched during the dragging process of the press board production, affecting the surface quality. Therefore, it is very necessary to prepare a scratch-resistant formaldehyde-free impregnated decorative paper. Summary of the invention
[0003] In view of the shortcomings of the prior art, the present invention aims to provide an impregnation emulsion for scratch-resistant formaldehyde-free impregnated decorative paper and a preparation method thereof. In the present invention, nanoapatite is dispersed in the resin as a filler. Therefore, the introduced filler increases the surface hardness of the impregnated decorative paper without significantly affecting the viscosity of the adhesive system, thereby achieving a scratch-resistant effect.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] A scratch-resistant formaldehyde-free impregnated decorative paper impregnated emulsion, comprising the following components:
[0006] 50-70 parts of silicone modified polyurethane-acrylate resin, 30-40 parts of acrylamide monomer, 2-8 parts of nano-hydroxyapatite, 2-5 parts of curing agent, 0.01-0.03 parts of defoaming agent, 0.01-0.05 parts of substrate wetting agent, and 30-45 parts of deionized water.
[0007] The preparation method of the organosilicon-modified polyurethane-acrylate resin comprises the following steps:
[0008] S1. Add 20-40 parts of diol and 16-40 parts of diisocyanate to a reactor with a stirring and reflux device, and carry out a prepolymerization reaction under the protection of 99.9% nitrogen at a reaction temperature of 40-60°C and a reaction time of 0.5-1h to obtain a polyurethane prepolymer;
[0009] S2. Heat the polyurethane prepolymer to 65-80°C, add the chain extender to the prepolymer, the addition time is 10-20 minutes, the chain extension reaction time is 0.5-1.5 hours, and the stirring speed is 50-100r / min. Then cool down to 40-60°C, add 8-12 parts of hydrophilic agent, add it within 25-30 minutes, and the reaction time of this step is 0.5-1.5 hours;
[0010] S3. Cool to room temperature, add 2 to 5 parts of glacial acetic acid for neutralization, and use 1 to 3 parts of acetone to reduce viscosity. After the viscosity is appropriate, add 10-15 parts of deionized water and 1-3 parts of silicone, and shear at a high speed of 2000-4000r / min. Evaporate and remove acetone to obtain a silicone-modified polyurethane emulsion. The solid content of the emulsion is 33-37%, the particle size is 50-100nm, the viscosity is 50-100cp, and the molecular weight is 500-2000;
[0011] S4. Add 0.1-0.2 parts of aqueous ammonia and 25-40 parts of deionized water, 10-15 parts of acrylate soft monomer, 20-25 parts of acrylate hard monomer, 0.1-0.3 parts of initiator, 5-10 parts of anionic surfactant and 6-14 parts of nonionic surfactant to the reactor, keep stirring at room temperature at 150-200r / min for 7-10min, stop the reaction immediately after the blue light is emitted, and obtain a polyacrylate pre-emulsion;
[0012] S5. The remaining 20-25 parts of the acrylate soft monomer and 20-25 parts of the acrylate hard monomer are mixed uniformly, and at 75-85 ° C, the remaining amount of the initiator is added dropwise to the polyacrylate pre-emulsion, and the stirring speed is maintained at 150-240r / min, and the temperature is raised to 75-85 ° C, and the remaining 2-9 parts of the silicone are added dropwise, and the dripping is completed in 30-40min. After the completion of the reaction, the reaction is kept warm for 15-30min to obtain a silicone-modified acrylate emulsion, the solid content of the emulsion is 33-37%, the particle size is 50-100nm, the viscosity is 20-100cp, and the molecular weight is 300-2000;
[0013] S6. The prepared organosilicon-modified polyurethane emulsion and organosilicon-modified polyacrylate emulsion are mixed, and reacted at a temperature of 50-70° C. for 25-30 minutes to obtain organosilicon-modified polyurethane-acrylate resin.
[0014] Preferably, the acrylamide monomer is one or more of acrylamide, hydroxymethyl acrylamide and hydroxyethyl acrylamide; the curing agent is preferably aziridine; and the defoaming agent is preferably polyether silicone oil.
[0015] Preferably, the nano-hydroxyapatite has a particle size of 20-80 nm.
[0016] Preferably, the silicone-modified polyurethane-acrylate resin comprises the following components in parts by mass: 16-40 parts of diisocyanate, 20-40 parts of diol, 40-50 parts of acrylate hard monomer, 30-40 parts of acrylate soft monomer, 5-10 parts of hydroxy acrylic monomer, 0.1-0.5 parts of glacial acetic acid, 3-8 parts of chain extender, 8-12 parts of hydrophilic agent, 0.1-0.3 parts of initiator, 5-10 parts of anionic surfactant, 6-14 parts of nonionic surfactant, 5-10 parts of silicone, 40-60 parts of water, and 0.1-0.2 parts of ammonia water.
[0017] Preferably, the diol is one or more of polyethylene glycol, polypropylene glycol, and polyester diol; the diisocyanate includes one or more of isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate.
[0018] Preferably, the acrylate hard monomer includes one or more of methyl methacrylate, acrylic acid, methacrylic acid, and acrylonitrile; the acrylate soft monomer includes one or more of methyl acrylate, butyl acrylate, and n-octyl acrylate; the hydroxy acrylic monomer is one of hydroxyethyl acrylate, hydroxybutyl acrylate, and dihydroxypropyl acrylate.
[0019] Preferably, the chain extender is one of ethylene glycol, propylene glycol, and 1,4-butanediol; the hydrophilic agent is N-methyldiethanolamine; the initiator is a persulfate, preferably one of sodium persulfate, ammonium persulfate, and potassium persulfate; and the anionic surfactant is sodium dodecyl sulfate.
[0020] Preferably, the nonionic surfactant is one or more of NP-15, A-103, and X-405.
[0021] Preferably, the organosilicon comprises two or more of tetraethoxysilane, vinyltrimethoxysilane and methylγ-mercaptopropyldimethoxysilane.
[0022] A method for preparing an impregnating emulsion for scratch-resistant formaldehyde-free impregnated decorative paper comprises the following steps:
[0023] Add 30-40 parts of acrylamide monomer, 2-8 parts of nano-hydroxyapatite, 2-5 parts of curing agent, 0.01-0.03 parts of defoaming agent and 0.01-0.05 parts of substrate wetting agent into silicone modified polyurethane-acrylate resin, stir for 8-10 minutes at room temperature and 100-150r / min, and let stand to obtain the scratch-resistant formaldehyde-free impregnated decorative paper impregnating emulsion.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. All components of the prepared adhesive contain no free formaldehyde, and the adhesive product releases no free formaldehyde, thus achieving formaldehyde-free impregnation of decorative paper.
[0026] 2. Modifying the polyurethane-acrylate emulsion with silicone and appropriately increasing its solid content can increase the glue absorption of the impregnated decorative paper. The introduction of acrylamide monomers can achieve rapid penetration into the interlayer of the decorative base paper at room temperature, and self-crosslink and cure at high temperature, thereby increasing the interlayer bonding strength of the impregnated decorative paper.
[0027] 3. Nanoapatite is dispersed in the resin as a filler. The introduced filler increases the surface hardness of the impregnated decorative paper without having a significant effect on the viscosity of the adhesive system, thereby achieving a scratch-resistant effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a diagram showing the steps for preparing the organosilicon-modified polyurethane-acrylate resin of the present invention. DETAILED DESCRIPTION
[0029] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] See also Figure 1 , the present invention provides a technical solution:
[0031] Example 1
[0032] A method for preparing an impregnating emulsion for scratch-resistant formaldehyde-free impregnated decorative paper:
[0033] S1. Add 20 parts of diol and 16 parts of diisocyanate into a reactor equipped with a stirring and reflux device, and carry out a prepolymerization reaction under the protection of 99.9% nitrogen at a reaction temperature of 40°C and a reaction time of 0.5h to obtain a polyurethane prepolymer.
[0034] S2. Heat the polyurethane prepolymer to 65°C, add the chain extender to the prepolymer, add for 10 minutes, and the chain extension reaction lasts for 0.5 hours at a stirring speed of 50 r / min. Then cool to 40°C, add 8 parts of hydrophilic agent, and add it within 25 minutes. The reaction time of this step is 0.5 hours.
[0035] S3. Cool to room temperature, add 2 parts of glacial acetic acid for neutralization, and use 1 part of acetone to reduce the viscosity. After the viscosity is appropriate, add 10 parts of deionized water and 1 part of silicone, and shear at high speed. The shear speed is 2000r / min, and the acetone is evaporated to obtain a silicone-modified polyurethane emulsion; the solid content of the emulsion is 33%, the particle size is 50nm, the viscosity is 50cp, and the molecular weight is 500.
[0036] S4. Add 0.1 parts of aqueous ammonia and 25 parts of deionized water, 10 parts of acrylate soft monomer, 20 parts of acrylate hard monomer, 0.1 parts of initiator, 5 parts of anionic surfactant and 6 parts of nonionic surfactant to the reactor, keep stirring at room temperature at 150r / min for 7min, and stop the reaction immediately after the blue light is emitted to obtain a polyacrylate pre-emulsion;
[0037] S5. Evenly mix the remaining 20 parts of acrylic soft monomer and 20 parts of acrylic hard monomer, and add them dropwise to the polyacrylate pre-emulsion together with the remaining initiator at 75°C. Maintain the stirring speed at 150r / min, raise the temperature to 75°C, and start to dropwise add the remaining 2 parts of silicone. Add the remaining 2 parts in 30 minutes. After the addition is completed, keep the temperature for 15 minutes to obtain a silicone-modified acrylic emulsion. The solid content of the emulsion is 33%, the particle size is 50nm, the viscosity is 20cp, and the molecular weight is 300.
[0038] S6. The prepared organosilicon-modified polyurethane emulsion and organosilicon-modified polyacrylate emulsion are mixed, and reacted at a temperature of 50° C. for 25 minutes to obtain organosilicon-modified polyurethane-acrylate resin.
[0039] S7. Add 30 parts of acrylamide monomer, 2 parts of nano-hydroxyapatite, 2 parts of curing agent, 0.01 parts of defoaming agent, and 0.01 parts of substrate wetting agent to silicone-modified polyurethane-acrylate resin, stir for 8 minutes at room temperature and 100 r / min, and let it stand to obtain an impregnation emulsion for scratch-resistant formaldehyde-free impregnated decorative paper.
[0040] The base paper is impregnated and dried with the impregnated latex for scratch-resistant formaldehyde-free impregnated decorative paper to obtain impregnated adhesive film paper; the impregnated decorative paper is hot-pressed onto the surface of the artificial board to obtain the decorative paper veneered artificial board.
[0041] Example 2
[0042] A method for preparing an impregnating emulsion for scratch-resistant formaldehyde-free impregnated decorative paper:
[0043] S1. Add 40 parts of diol and 40 parts of diisocyanate into a reactor equipped with a stirring and reflux device, and carry out a prepolymerization reaction under the protection of 99.9% nitrogen at a reaction temperature of 60°C and a reaction time of 1 hour to obtain a polyurethane prepolymer.
[0044] S2. Heat the polyurethane prepolymer to 80°C, add the chain extender to the prepolymer, add for 20 minutes, and the chain extension reaction lasts for 1.5 hours at a stirring speed of 100 r / min. Then cool to 60°C, add 12 parts of hydrophilic agent, and add it within 30 minutes. The reaction time of this step is 1.5 hours.
[0045] S3. Cool to room temperature, add 5 parts of glacial acetic acid for neutralization, and use 3 parts of acetone to reduce the viscosity. After the viscosity is appropriate, add 15 parts of deionized water and 3 parts of silicone, and shear at a high speed of 4000r / min. Evaporate and remove acetone to obtain silicone-modified polyurethane emulsion; the solid content of the emulsion is 37%, the particle size is 100nm, the viscosity is 100cp, and the molecular weight is 2000.
[0046] S4. 0.2 parts of aqueous ammonia and 40 parts of deionized water, 15 parts of acrylate soft monomer, 25 parts of acrylate hard monomer, 0.3 parts of initiator, 10 parts of anionic surfactant and 14 parts of nonionic surfactant were added to the reactor, and the stirring speed was maintained at room temperature at 200r / min for 10min. The reaction was stopped immediately after the blue light was emitted to obtain a polyacrylate pre-emulsion;
[0047] S5. Evenly mix the remaining 25 parts of acrylic soft monomer and 25 parts of acrylic hard monomer, and add them dropwise to the polyacrylate pre-emulsion together with the remaining initiator at 85°C, keep the stirring speed at 240r / min, raise the temperature to 85°C, start to add the remaining 9 parts of silicone, and finish adding in 40 minutes. After completion, keep the temperature and react for 30 minutes to obtain silicone-modified acrylic emulsion; the solid content of the emulsion is 37%, the particle size is 100nm, the viscosity is 100cp, and the molecular weight is 2000.
[0048] S6. The prepared organosilicon-modified polyurethane emulsion and organosilicon-modified polyacrylate emulsion are mixed, and reacted at a temperature of 70° C. for 30 minutes to obtain organosilicon-modified polyurethane-acrylate resin.
[0049] S7. Add 40 parts of acrylamide monomer, 8 parts of nano-hydroxyapatite, 5 parts of curing agent, 0.03 parts of defoaming agent, and 0.05 parts of substrate wetting agent to silicone-modified polyurethane-acrylate resin, stir for 10 minutes at room temperature and 150 r / min, and let it stand to obtain an impregnation emulsion for scratch-resistant formaldehyde-free impregnated decorative paper.
[0050] The base paper is impregnated and dried with the impregnated latex for scratch-resistant formaldehyde-free impregnated decorative paper to obtain impregnated adhesive film paper; the impregnated decorative paper is hot-pressed onto the surface of the artificial board to obtain the decorative paper veneered artificial board.
[0051] Example 3
[0052] A method for preparing an impregnating emulsion for scratch-resistant formaldehyde-free impregnated decorative paper:
[0053] S1. Add 30 parts of diol and 30 parts of diisocyanate into a reactor equipped with a stirring and reflux device, and carry out a prepolymerization reaction under the protection of 99.9% nitrogen at a reaction temperature of 50°C and a reaction time of 0.7h to obtain a polyurethane prepolymer.
[0054] S2. Heat the polyurethane prepolymer to 70°C, add the chain extender to the prepolymer, add for 15 minutes, and the chain extension reaction lasts for 1 hour, with a stirring speed of 70r / min. Then cool to 40-60°C, add 9 parts of hydrophilic agent, and add it within 27 minutes. The reaction time of this step is 1.0 hour.
[0055] S3. Cool to room temperature, add 3 parts of glacial acetic acid for neutralization, and use 2 parts of acetone to reduce the viscosity. After the viscosity is appropriate, add 12 parts of deionized water and 2 parts of silicone, and shear at high speed. The shear speed is 3000r / min, and the acetone is evaporated to obtain a silicone-modified polyurethane emulsion; the solid content of the emulsion is 35%, the particle size is 75nm, the viscosity is 70, and the molecular weight is 1500.
[0056] S4. 0.15 parts of aqueous ammonia and 30 parts of deionized water, 12 parts of acrylate soft monomer, 22 parts of acrylate hard monomer, 0.2 parts of initiator, 7 parts of anionic surfactant and 9 parts of nonionic surfactant were added to the reactor, and the stirring speed was maintained at room temperature for 8 minutes at 175r / min. The reaction was stopped immediately after the blue light was emitted to obtain a polyacrylate pre-emulsion;
[0057] S5. Evenly mix the remaining 22 parts of acrylic soft monomer and 22 parts of acrylic hard monomer, and add them dropwise to the polyacrylate pre-emulsion together with the remaining initiator at 79°C, keep the stirring speed at 200r / min, raise the temperature to 79°C, start to add the remaining 5 parts of silicone, and finish adding in 35 minutes. After completion, keep the temperature and react for 17 minutes to obtain silicone-modified acrylic emulsion; the solid content of the emulsion is 35%, the particle size is 75nm, the viscosity is 50cp, and the molecular weight is 900.
[0058] S6. The prepared organosilicon-modified polyurethane emulsion and organosilicon-modified polyacrylate emulsion were mixed and reacted at a temperature of 60° C. for 27 minutes to obtain organosilicon-modified polyurethane-acrylate resin.
[0059] S7. Add 35 parts of acrylamide monomer, 4 parts of nano-hydroxyapatite, 2-5 parts of curing agent, 0.02 parts of defoaming agent, and 0.03 parts of substrate wetting agent to silicone-modified polyurethane-acrylate resin, stir for 9 minutes at room temperature and 125 r / min, and let it stand to obtain the scratch-resistant formaldehyde-free impregnated decorative paper impregnating emulsion for decorative paper.
[0060] The base paper is impregnated and dried with the impregnated latex for scratch-resistant formaldehyde-free impregnated decorative paper to obtain impregnated adhesive film paper; the impregnated decorative paper is hot-pressed onto the surface of the artificial board to obtain the decorative paper veneered artificial board.
[0061] Example 4
[0062] A method for preparing an impregnating emulsion for scratch-resistant formaldehyde-free impregnated decorative paper:
[0063] S1. Add 35 parts of diol and 35 parts of diisocyanate into a reactor equipped with a stirring and reflux device, and carry out a prepolymerization reaction under the protection of 99.9% nitrogen at a reaction temperature of 55°C and a reaction time of 0.8h to obtain a polyurethane prepolymer.
[0064] S2. Heat the polyurethane prepolymer to 75°C, add the chain extender to the prepolymer, add for 18 minutes, and the chain extension reaction lasts for 1.4 hours at a stirring speed of 80r / min. Then cool to 55°C, add 11 parts of hydrophilic agent, and add it within 29 minutes. The reaction time of this step is 1.4 hours.
[0065] S3. Cool to room temperature, add 4 parts of glacial acetic acid for neutralization, and use 2 parts of acetone to reduce the viscosity. After the viscosity is appropriate, add 14 parts of deionized water and 2.5 parts of silicone, and shear at high speed. The shear speed is 3500r / min, and the acetone is evaporated to obtain a silicone-modified polyurethane emulsion; the solid content of the emulsion is 36%, the particle size is 90nm, the viscosity is 90cp, and the molecular weight is 1500.
[0066] S4. 0.15 parts of aqueous ammonia and 35 parts of deionized water, 14 parts of acrylate soft monomer, 24 parts of acrylate hard monomer, 0.25 parts of initiator, 9 parts of anionic surfactant and 13 parts of nonionic surfactant were added to the reactor, and the stirring speed was maintained at room temperature for 9 minutes at 190r / min. The reaction was stopped immediately after the blue light was emitted to obtain a polyacrylate pre-emulsion;
[0067] S5. The remaining 24 parts of acrylate soft monomer and 24 parts of acrylate hard monomer are mixed evenly, and at 83°C, they are added dropwise to the polyacrylate pre-emulsion together with the remaining initiator, and the temperature is raised to 75-85°C while maintaining a stirring speed of 150-240r / min. The remaining 2-9 parts of silicone are added dropwise, and the addition is completed within 30-40 minutes. After the addition is completed, the reaction is kept warm for 15-30 minutes to obtain a silicone-modified acrylate emulsion; the solid content of the emulsion is 33-37%, the particle size is 50-100nm, the viscosity is 20-100cp, and the molecular weight is 300-2000.
[0068] S6. The prepared organosilicon-modified polyurethane emulsion and organosilicon-modified polyacrylate emulsion are mixed, and reacted at a temperature of 50-70° C. for 25-30 minutes to obtain organosilicon-modified polyurethane-acrylate resin.
[0069] S7. Add 30-40 parts of acrylamide monomer, 2-8 parts of nano-hydroxyapatite, 2-5 parts of curing agent, 0.01-0.03 parts of defoaming agent, and 0.01-0.05 parts of substrate wetting agent to silicone-modified polyurethane-acrylate resin, stir for 8-10 minutes at room temperature and 100-150 r / min, and let it stand to obtain an impregnation emulsion for scratch-resistant formaldehyde-free impregnated decorative paper.
[0070] The base paper is impregnated and dried with the impregnated latex for scratch-resistant formaldehyde-free impregnated decorative paper to obtain impregnated adhesive film paper; the impregnated decorative paper is hot-pressed onto the surface of the artificial board to obtain the decorative paper veneered artificial board.
[0071] Comparative Example 1
[0072] The impregnation resin system in Example 1 described in ZL202010394895.7 is used to impregnate the decorative base paper to obtain impregnated film paper; the impregnated decorative paper is hot-pressed onto the surface of the artificial board to obtain the decorative paper veneered artificial board.
[0073] Comparative Example 2
[0074] The impregnation resin system of Example 1 described in ZL202010394935.8 is used to impregnate the decorative base paper to obtain impregnated film paper; the impregnated decorative paper is hot-pressed onto the surface of the artificial board to obtain the decorative paper veneered artificial board.
[0075] Performance Test:
[0076] Referring to the national standards: GB / T 28995-2012 and GB / T 15102-2017, the physical properties of the impregnated decorative paper of Examples 1-4 and Comparative Examples 1-2 were tested. The test results are shown in Table 1 below:
[0077] Table 1 Comparison of physical properties of decorative paper and veneer board after impregnation
[0078]
[0079]
[0080] Compared with the published comparative examples 1 and 2 of the formaldehyde-free adhesive for decorative paper, the decorative paper examples 1-4 prepared by the impregnation emulsion for scratch-resistant formaldehyde-free impregnated decorative paper of the present invention not only do not release free formaldehyde, but also have a higher amount of adhesive, better paper permeability, better surface bonding strength, scratch resistance and wear resistance of the decorative panel, and all meet the requirements of relevant national standards. The organic silicon in the adhesive formula reduces the particle size and adhesiveness of the impregnated adhesive, and the nano-hydroxyapatite is used as a reinforcing material to increase the amount of adhesive absorption and surface hardness of the formaldehyde-free impregnated decorative paper, thereby achieving the anti-scratch effect.
[0081] Funded project: National Key R&D Program Project "Preparation and Application of Green Decorative Materials on the Surface of Wood Products" (2025YFD2200703).
[0082] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An impregnation emulsion for scratch-resistant formaldehyde-free impregnated decorative paper, characterized in that: Includes the following components: 50-70 parts of silicone modified polyurethane-acrylate resin, 30-40 parts of acrylamide monomer, 2-8 parts of nano-hydroxyapatite, 2-5 parts of curing agent, 0.01-0.03 parts of defoaming agent, 0.01-0.05 parts of substrate wetting agent, and 30-45 parts of deionized water. The preparation method of the organosilicon-modified polyurethane-acrylate resin comprises the following steps: S1. Add 20-40 parts of diol and 16-40 parts of diisocyanate to a reactor with a stirring and reflux device, and carry out a prepolymerization reaction under the protection of 99.9% nitrogen at a reaction temperature of 40-60°C and a reaction time of 0.5-1h to obtain a polyurethane prepolymer; S2. Heat the polyurethane prepolymer to 65-80°C, add the chain extender to the prepolymer, the addition time is 10-20 minutes, the chain extension reaction time is 0.5-1.5 hours, and the stirring speed is 50-100r / min. Then cool down to 40-60°C, add 8-12 parts of hydrophilic agent, add it within 25-30 minutes, and the reaction time of this step is 0.5-1.5 hours; S3. Cool to room temperature, add 2 to 5 parts of glacial acetic acid for neutralization, and use 1 to 3 parts of acetone to reduce viscosity. After the viscosity is appropriate, add 10-15 parts of deionized water and 1-3 parts of silicone, and shear at a high speed of 2000-4000r / min. Evaporate and remove acetone to obtain a silicone-modified polyurethane emulsion. The solid content of the emulsion is 33-37%, the particle size is 50-100nm, the viscosity is 50-100cp, and the molecular weight is 500-2000; S4. Add 0.1-0.2 parts of aqueous ammonia and 25-40 parts of deionized water, 10-15 parts of acrylate soft monomer, 20-25 parts of acrylate hard monomer, 0.1-0.3 parts of initiator, 5-10 parts of anionic surfactant and 6-14 parts of nonionic surfactant to the reactor, keep stirring at room temperature at 150-200r / min for 7-10min, stop the reaction immediately after the blue light is emitted, and obtain a polyacrylate pre-emulsion; S5. The remaining 20-25 parts of the acrylate soft monomer and 20-25 parts of the acrylate hard monomer are mixed uniformly, and at 75-85 ° C, the remaining amount of the initiator is added dropwise to the polyacrylate pre-emulsion, and the stirring speed is maintained at 150-240r / min, and the temperature is raised to 75-85 ° C, and the remaining 2-9 parts of the silicone are added dropwise, and the dripping is completed in 30-40min. After the completion of the reaction, the reaction is kept warm for 15-30min to obtain a silicone-modified acrylate emulsion, the solid content of the emulsion is 33-37%, the particle size is 50-100nm, the viscosity is 20-100cp, and the molecular weight is 300-2000; S6. The prepared organosilicon-modified polyurethane emulsion and organosilicon-modified polyacrylate emulsion are mixed, and reacted at a temperature of 50-70° C. for 25-30 minutes to obtain organosilicon-modified polyurethane-acrylate resin.
2. The scratch-resistant formaldehyde-free impregnated decorative paper according to claim 1, characterized in that: The acrylamide monomer is one or more of acrylamide, hydroxymethyl acrylamide and hydroxyethyl acrylamide; the curing agent is preferably aziridine; and the defoaming agent is preferably polyether silicone oil.
3. The scratch-resistant formaldehyde-free impregnated decorative paper according to claim 1, characterized in that: The nano-hydroxyapatite has a particle size of 20-80 nm.
4. The impregnation emulsion for scratch-resistant formaldehyde-free impregnated decorative paper according to claim 1, characterized in that: The organosilicon-modified polyurethane-acrylate resin comprises the following components in parts by mass: 16-40 parts of diisocyanate, 20-40 parts of diol, 40-50 parts of acrylate hard monomer, 30-40 parts of acrylate soft monomer, 5-10 parts of hydroxy acrylic monomer, 0.1-0.5 parts of glacial acetic acid, 3-8 parts of chain extender, 8-12 parts of hydrophilic agent, 0.1-0.3 parts of initiator, 5-10 parts of anionic surfactant, 6-14 parts of nonionic surfactant, 5-10 parts of organosilicon, 40-60 parts of water and 0.1-0.2 parts of ammonia water.
5. The scratch-resistant formaldehyde-free impregnated decorative paper impregnated emulsion according to claim 4, characterized in that: The diol is one or more of polyethylene glycol, polypropylene glycol, and polyester diol; the diisocyanate includes one or more of isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate.
6. The scratch-resistant formaldehyde-free impregnated decorative paper according to claim 4, characterized in that: The hard acrylate monomer includes one or more of methyl methacrylate, acrylic acid, methacrylic acid, and acrylonitrile; the soft acrylate monomer includes one or more of methyl acrylate, butyl acrylate, and n-octyl acrylate; the hydroxy acrylic monomer is one of hydroxyethyl acrylate, hydroxybutyl acrylate, and dihydroxypropyl acrylate.
7. The impregnation emulsion for scratch-resistant formaldehyde-free impregnated decorative paper according to claim 4, characterized in that: The chain extender is one of ethylene glycol, propylene glycol and 1,4-butanediol; the hydrophilic agent is N-methyldiethanolamine; the initiator is a persulfate, preferably one of sodium persulfate, ammonium persulfate and potassium persulfate; and the anionic surfactant is sodium dodecyl sulfate.
8. The scratch-resistant formaldehyde-free impregnated decorative paper according to claim 4, characterized in that: The nonionic surfactant is one or more of NP-15, A-103, and X-405.
9. The impregnation emulsion for scratch-resistant formaldehyde-free impregnated decorative paper according to claim 4, characterized in that: The organic silicon comprises two or more of tetraethoxysilane, vinyltrimethoxysilane and methylγ-mercaptopropyldimethoxysilane.
10. The method for preparing the scratch-resistant formaldehyde-free impregnated decorative paper according to claim 1, characterized in that: The following steps are involved: Add 30-40 parts of acrylamide monomer, 2-8 parts of nano-hydroxyapatite, 2-5 parts of curing agent, 0.01-0.03 parts of defoaming agent and 0.01-0.05 parts of substrate wetting agent into silicone modified polyurethane-acrylate resin, stir for 8-10 minutes at room temperature and 100-150r / min, and let stand to obtain the scratch-resistant formaldehyde-free impregnated decorative paper impregnating emulsion.
Citation Information
Patent Citations
Formaldehyde-free decorative adhesive film paper and preparation method thereof
CN109457536A
Formaldehyde-free adhesive for paper impregnated thermosetting resin and preparation method of adhesive
CN111411543A
Formaldehyde-free impregnated adhesive for decorative paper and preparation method of formaldehyde-free impregnated adhesive
CN111501416A