Damp-proof environment-friendly construction method for building outer wall
By laying waterproof membranes on the exterior walls of buildings, applying waterproof mortar, and spraying waterproof coatings, a multi-layered waterproof barrier is formed using composite sulfides and nanoparticles, solving the problem of poor moisture-proof performance and durability of building exterior walls, and achieving a highly efficient and environmentally friendly moisture-proof effect.
Patent Information
- Application Number
- CN202410951462.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-22
AI Technical Summary
Existing building exterior walls have poor moisture-proof, durability, and environmental performance. Traditional construction methods suffer from problems such as environmentally unfriendly materials, low construction efficiency, and unsatisfactory moisture-proof effects.
A waterproofing agent is prepared by combining composite sulfides and hydroxylated hexagonal boron nitride nanoparticles, and a waterproof coating is prepared by combining hexachlorocyclotriphosphazene, hexafluoroisopropanol, trifluoroethanol and nano silica particles. A multi-layer waterproof barrier is formed by laying waterproof membranes, applying waterproof mortar and spraying waterproof coatings on the exterior walls of buildings.
It significantly improves the moisture-proof, mechanical, and environmental performance of building exterior walls, forming a continuous waterproof layer, enhancing adhesion and impermeability, extending service life, preventing water penetration, and the material is environmentally friendly and stable.
Smart Images

Figure CN118997530A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building exterior wall construction, and in particular relates to a moisture-proof and environmentally friendly construction method for building exterior walls. Background Art
[0002] With the acceleration of urbanization, the number of buildings has increased sharply, but the resulting environmental and building quality problems have also become increasingly prominent. Among them, the moisture-proof performance of the building's exterior walls is directly related to the service life of the building and the comfort of the residents. Traditional moisture-proof construction methods often have problems such as environmentally unfriendly materials, low construction efficiency, and unsatisfactory moisture-proof effects.
[0003] In this context, it is particularly important to study a method for building exterior wall construction that is both moisture-proof and environmentally friendly. This method aims to achieve efficient moisture-proofing and environmental protection of building exterior walls by selecting low-pollution, renewable or recyclable environmentally friendly materials and combining advanced construction processes and technical means. At the same time, with the continuous advancement of science and technology, the continuous emergence of new waterproof materials and moisture-proof technologies has also provided strong support for the research of this construction method. Therefore, a moisture-proof and environmentally friendly construction method for building exterior walls has both the internal needs of industry development and the external impetus of scientific and technological progress and market demand. The research on this method will not only help improve the moisture-proof performance and living quality of buildings, but also help promote the green development and sustainable development of the construction industry.
[0004] Patent CN 212689300 U discloses an energy-saving and moisture-proof building exterior wall, including an exterior wall body, and also including an installation groove opened on the outside of the exterior wall body, an insulation board is installed in the installation groove, the installation groove penetrates the exterior wall body along the height direction of the exterior wall body and the width of the installation groove gradually decreases from top to bottom, the outside of the installation groove is provided with two abutting edges for limiting the movement of the insulation board along the thickness direction of the exterior wall body, a wall reinforcement layer is installed on the side of the insulation board away from the exterior wall body, the wall reinforcement layer is located between the two abutting edges, a waterproof coil is attached to the outside of the wall reinforcement layer, and a waterproofing component is provided on the side of the waterproof coil away from the exterior wall body. The invention can effectively reduce moisture infiltration into the wall, but the moisture-proof performance, durability and environmental protection performance of the wall still have room for improvement. Summary of the invention
[0005] The object of the present invention is to provide an environmentally friendly moisture-proof construction method for building exterior walls, which is used to solve the technical problems of poor moisture-proof performance, durability and environmental protection performance of the wall in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a moisture-proof environmentally friendly construction method for building exterior walls, comprising the following steps:
[0008] Step (1): Clean the surface of the base layer to remove dust, moss and oil stains, and then repair cracks and holes to ensure that the surface of the base layer is flat, clean and free of defects to obtain a building base layer;
[0009] Step (2): laying a waterproofing membrane on the surface of a building base using a hot melt method to obtain a base treated with the waterproofing membrane;
[0010] Step (3): evenly apply the asphalt coating on the surface of the base treated with the waterproof membrane, and then apply the waterproof mortar, apply it multiple times to obtain a building base containing mortar;
[0011] Step (4): After mixing the waterproof coating with water, spray it on the surface of the building base containing mortar, and after drying, paste tiles to obtain a moisture-proof building exterior wall.
[0012] Preferably, in step (2), when laying the waterproof membrane, the end portion of the membrane is sealed.
[0013] Preferably, in step (3), the method for preparing the waterproof mortar comprises the following steps:
[0014] Q1: Add chloropropyltriethoxysilane, cystamine sulfate, potassium carbonate, potassium iodide and anhydrous toluene into a dry container, introduce nitrogen to expel oxygen, heat and react under the protection of nitrogen atmosphere, and after the reaction is completed, filter, rotary evaporate and vacuum dry to obtain a composite sulfide;
[0015] Q2: placing hexagonal boron nitride in a mixed solution of isopropanol and deionized water, placing it in an ultrasonic cleaner for ultrasonic stripping after ultrasonic treatment, and after the stripping is completed, centrifuging the mixed solution, vacuum filtering, and vacuum drying to obtain hydroxylated hexagonal boron nitride nanoparticles;
[0016] Q3: Add hydroxylated hexagonal boron nitride nanoparticles to a mixed solution of ethanol and deionized water, disperse by ultrasonication, then add the composite sulfide, stir, condense and reflux under oil bath conditions, cool, filter, wash and dry to obtain a waterproofing agent;
[0017] Q4: Mix cement, sand, water and waterproofing agent to obtain waterproof mortar.
[0018] In the above process, the synthetic reaction formula of the waterproofing agent is as follows:
[0019]
[0020] The results of mass spectrometry analysis were: m / z: 1075.29 (100.0%), 1076.28 (58.4%), 1074.29 (57.1%), 1076.29 (41.1%), 1077.28 (40.2%), 1078.28 (31.1%), 1077.29 (24.7%), 1073.29 (21.0%), 1079.28 (13.5%), 1078.29 (8 .7%), 1074.30(5.8%), 1072.30(5.5%), 1080.28(4.4%), 1079.29(3.8%), 1075.30(3.2%), 1073.30(2.6%), 1080.27(2.4%), 1076.30(2.1%), 1081.28(1.5%), 1077.30(1.2%), 1080.29(1.1%).
[0021] Preferably, in Q1, the molar ratio of chloropropyltriethoxysilane, cystamine sulfate, potassium carbonate and potassium iodide is (0.5-1.0): (0.6-1.2): (1.5-3): (0.05-0.1), the heating reaction temperature is 70-80°C, the heating reaction time is 20-24h, the vacuum drying temperature is 50-60°C, and the time is 20-24h; in Q2, the amount ratio of hexagonal boron nitride, isopropanol and deionized water is (1.5-2.0) g: (150-200) mL: (150-200) mL, the ultrasonic treatment time is 1-2h, the stripping time is 10-12h, the centrifugal speed is 4000-5000rpm, the centrifugal time is 30-45min, the vacuum drying temperature is 90-110°C, and the time is 10-12h.
[0022] Preferably, in Q3, the dosage ratio of hydroxylated hexagonal boron nitride nanoparticles, ethanol, deionized water and complex sulfide is (0.2-0.4) g: (150-300) mL: (50-100) mL: (0.5-1) mL, the ultrasonic dispersion time is 1-2 h, the oil bath temperature is 90-110° C., and the condensation reflux time is 20-24 h; in Q4, the dosage ratio of cement, sand, water and waterproofing agent is (1-3) kg: (2-6) kg: (500-600) mL: (0.05-0.15) kg, and the mixing and stirring time is 10-12 h.
[0023] Preferably, in step (4), the method for preparing the waterproof coating comprises the following steps:
[0024] S1: adding hexachlorocyclotriphosphazene to a container containing chloronaphthalene, heating and stirring to react, adding palladium after the hexachlorocyclotriphosphazene is completely dissolved, condensing and refluxing, stopping heating after the reaction is completed, cooling, and pouring the solution into petroleum ether and stirring to obtain product 1;
[0025] S2: adding hexafluoroisopropanol to tetrahydrofuran containing metallic sodium using a constant pressure dropping funnel to obtain a mixed solution A; adding trifluoroethanol and octafluoropentanol to tetrahydrofuran containing metallic sodium to obtain a mixed solution B; adding the intermediate product 1 to tetrahydrofuran containing metallic sodium using a constant pressure dropping funnel to obtain a mixed solution C;
[0026] S3: under ice bath conditions, the mixed solution A and the mixed solution B are added dropwise to the mixed solution C. After the addition is completed, the reaction is continued, and the product 2 is obtained by washing and drying.
[0027] S4: Add product 2 to tetrahydrofuran, stir, and ultrasonically treat, then add nano-silica particles, and vacuum dry to obtain a waterproof coating.
[0028] In the above process, the synthetic reaction formula of product 2 is as follows:
[0029]
[0030] Preferably, in S1, the dosage ratio of hexachlorocyclotriphosphazene, chloronaphthalene and palladium is (8-10) g: (5-8) mL: (0.05-0.08) g, the heating temperature is 120-140° C., the condensation reflux time is 8-10 h, the cooling temperature is 90-100° C., and the stirring time is 2-3 h.
[0031] Preferably, in S2, the molar ratio of hexafluoroisopropanol and metallic sodium is (0.8-1.1):(0.9-1.2), the molar ratio of trifluoroethanol, octafluoropentanol and metallic sodium is (0.3-0.5):(1.1-1.3):(1.4-1.8), and the molar ratio of the intermediate product 1 and metallic sodium is (0.3-0.5):(0.3-0.5).
[0032] Preferably, in S3, the volume ratio of mixed solution A, mixed solution B and mixed solution C is (0.35-0.7):(1.15-2.30):(1-2), the reaction time is continued for 10-12 hours, first washed with petroleum ether and deionized water in two phases, and then washed with deionized water, the drying temperature is 60-70°C, and the time is 8-10 hours.
[0033] Preferably, in S4, the mass ratio of product 2 to nano-silica particles is (10-20): (1-2), the stirring time is 30-45 min, the ultrasonic treatment time is 30-60 min, the vacuum drying temperature is 60-70°C, and the time is 4-6 h.
[0034] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0035] 1. The present invention first combines composite sulfide with hydroxylated hexagonal boron nitride nanoparticles to prepare a waterproof agent, and adds the composite sulfide to cement and sand to prepare a waterproof mortar, which is evenly applied on the surface of a waterproof roll material to effectively improve the moisture-proof performance and mechanical properties of a building exterior wall. Subsequently, hexachlorocyclotriphosphazene, hexafluoroisopropanol, trifluoroethanol, octafluoropentanol and nano-silica particles are used as raw materials to prepare a waterproof coating, which is used in the building exterior wall to effectively improve the moisture-proof performance and durability of the building exterior wall. Therefore, the building exterior wall using the waterproof mortar and the waterproof coating has excellent moisture-proof performance, durability and environmental protection.
[0036] 2. The present invention uses chloropropyltriethoxysilane, cystamine sulfate, hexagonal boron nitride, cement and sand as raw materials to obtain waterproof mortar, which is applied on the surface of waterproof coiled material to effectively improve the moisture-proof performance, mechanical properties, adhesion and durability of the building exterior wall. The composite sulfide and hydroxylated hexagonal boron nitride nanoparticles in the waterproof mortar together constitute an effective waterproof barrier. The composite sulfide itself is hydrophobic and can form a continuous waterproof layer in the mortar. The nano-scale size effect contained in the hydroxylated hexagonal boron nitride nanoparticles and the hydroxyl groups on the surface can significantly enhance the density and impermeability of the mortar, making it difficult for water to penetrate. The chloropropyltriethoxysilane reacts with the inorganic components in the mortar to form an organic-inorganic hybrid network structure. The existence of this structure can effectively improve the cohesive strength of the mortar and enhance its mechanical properties. A bonding reaction will occur between the waterproofing agent in the waterproof mortar and the waterproof membrane to form a strong chemical bond, thereby enhancing the adhesion between the waterproof mortar and the waterproof membrane. The excellent thermal stability and chemical stability of hexagonal boron nitride nanoparticles can extend the service life of the waterproof mortar and delay the aging process of the waterproof mortar, thereby giving the building exterior wall excellent moisture-proof and durability.
[0037] 3. The present invention uses hexachlorocyclotriphosphazene, hexafluoroisopropyl ketone, trifluoroethanol, octafluoropentanol and nano-silica particles as raw materials to prepare a waterproof coating. The waterproof coating is used in building exterior walls to effectively improve its moisture resistance, durability and environmental protection. The hexachlorocyclotriphosphazene and its derivatives in the waterproof coating can form a waterproof film in the coating, which effectively prevents moisture penetration through physical barrier and chemical stability. The addition of hexafluoroisopropyl ketone, trifluoroethanol and octafluoropentanol can improve the film-forming property and permeability of the coating, and further enhance the waterproof performance. The hexachlorocyclotriphosphazene and nano-silica particles present in the waterproof coating have excellent weather resistance and chemical corrosion resistance, so that the prepared waterproof coating has excellent stability and is not easily damaged or degraded. The prepared waterproof coating is mainly composed of organic and inorganic compounds, is relatively stable in the environment, is not easy to decompose and produce harmful substances, and is fixed in the coating during use, and has excellent safety performance and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0039] Figure 1 It is a cross-sectional schematic diagram of the moisture-proof building exterior wall of the present invention;
[0040] Figure 2 It is a front view of the moisture-proof building exterior wall of the present invention.
[0041] Description of the drawings: 1. Building base layer; 2. Waterproof membrane layer; 3. Waterproof mortar layer; 4. Waterproof coating layer; 5. Ceramic tile layer. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Example 1
[0044] See also Figure 1 and Figure 2As shown, the moisture-proof building exterior wall layer obtained by the construction of the present invention includes a building base layer 1, a waterproof coiled material layer 2, a waterproof mortar layer 3, a waterproof coating layer 4 and a ceramic tile layer 5. The five-layer structure is tightly fitted from the inside to the outside, one side of the waterproof coiled material layer 2 is tightly fitted to the building base layer 1, and the other side is tightly connected to the waterproof mortar layer 3, the other side of the waterproof mortar layer 3 is tightly connected to the waterproof coating layer 4, and the other side of the waterproof coating layer 4 is tightly fitted to the ceramic tile layer 5 to form a moisture-proof building exterior wall. The building exterior wall obtained by this method not only has excellent moisture-proof performance, but also has excellent environmental protection and thermal insulation properties.
[0045] Example 2
[0046] This embodiment discloses a method for preparing a waterproof mortar, comprising the following steps:
[0047] Q1: 1.5 g of chloropropyltriethoxysilane, 1.88 g of cystamine sulfate, 2.56 g of potassium carbonate, 0.10 g of potassium iodide and 6 mL of anhydrous toluene were added to a dry container, nitrogen was introduced to expel oxygen, and the mixture was heated at 80°C for 24 h under the protection of nitrogen atmosphere. After the reaction was completed, the mixture was filtered, rotary evaporated, and vacuum dried at 60°C for 24 h to obtain a composite sulfide;
[0048] Q2: 1.75 g of hexagonal boron nitride was placed in a mixed solution of 175 mL of isopropanol and 175 mL of deionized water, and ultrasonically treated for 2 h, and then placed in an ultrasonic cleaner for ultrasonic stripping for 12 h. After the stripping, the mixed solution was centrifuged at 5000 rpm for 35 min, vacuum filtered, and vacuum dried at 90 ° C for 12 h to obtain hydroxylated hexagonal boron nitride nanoparticles;
[0049] Q3: 0.3 g of hydroxylated hexagonal boron nitride nanoparticles was added to a mixed solution of 225 mL of ethanol and 75 mL of deionized water, and ultrasonically dispersed for 2 h. Then, 0.75 mL of complex sulfide was added, and the mixture was stirred, condensed and refluxed for 24 h under 100 °C oil bath conditions. The mixture was cooled, filtered, washed and dried to obtain a waterproofing agent.
[0050] Q4: Mix 2kg cement, 4kg sand, 550mL water and 0.1kg waterproofing agent and stir for 12h to obtain waterproof mortar.
[0051] This embodiment discloses a method for preparing a waterproof coating, comprising the following steps:
[0052] S1: Add 9 g of hexachlorocyclotriphosphazene to a container containing 6.5 mL of naphthalene chloride, heat to 140°C and stir to react. After the hexachlorocyclotriphosphazene is completely dissolved, add 0.06 g of palladium, condense and reflux for 10 h. After the reaction is completed, stop heating, cool to 100°C, pour the solution into petroleum ether and stir for 3 h to obtain product 1;
[0053] S2: 4.84 mL of hexafluoroisopropanol was added dropwise to 15 mL of tetrahydrofuran containing 1.16 g of metallic sodium using a constant pressure dropping funnel to obtain a mixed solution A; 1.34 g of trifluoroethanol and 9.28 g of octafluoropentanol were added to 15 mL of tetrahydrofuran containing 1.23 g of metallic sodium to obtain a mixed solution B; 7.19 g of the intermediate product 1 was added to 15 mL of tetrahydrofuran containing 1.35 g of metallic sodium using a constant pressure dropping funnel to obtain a mixed solution C;
[0054] S3: Under ice bath conditions, 52 mL of mixed solution A and 173 mL of mixed solution B were added dropwise to 150 mL of mixed solution C. After the addition was completed, the reaction was continued for 12 h. The mixture was first washed with petroleum ether and deionized water in two phases, then washed with deionized water, and dried at 70 °C for 8 h to obtain product 2.
[0055] S4: Add 15 g of product 2 to 30 mL of tetrahydrofuran, stir for 30 min, ultrasonically treat for 45 min, then add 1.5 g of nano-silica particles, and vacuum dry at 70° C. for 4 h to obtain a waterproof coating.
[0056] This embodiment discloses a moisture-proof environmentally friendly construction method for building exterior walls, comprising the following steps:
[0057] Step (1): Clean the surface of the base layer to remove dust, moss and oil stains, and then repair cracks and holes to ensure that the surface of the base layer is flat, clean and free of defects to obtain a building base layer;
[0058] Step (2): using a hot melt method to lay a waterproofing membrane on the surface of a building base layer, and when laying the waterproofing membrane, sealing the end of the membrane to obtain a base layer treated with the waterproofing membrane;
[0059] Step (3): evenly apply the asphalt coating on the surface of the base treated with the waterproof membrane, and then apply the waterproof mortar, apply it multiple times to obtain a building base containing mortar;
[0060] Step (4): After mixing the waterproof coating with water, spray it on the surface of the building base containing mortar, and after drying, paste tiles to obtain a moisture-proof building exterior wall.
[0061] Example 3
[0062] This embodiment discloses a method for preparing a waterproof mortar, comprising the following steps:
[0063] Q1: 1.0 g of chloropropyltriethoxysilane, 1.25 g of cystamine sulfate, 1.72 g of potassium carbonate, 0.07 g of potassium iodide and 6 mL of anhydrous toluene were added to a dry container, nitrogen was introduced to expel oxygen, and the mixture was heated at 80°C for 24 h under the protection of nitrogen atmosphere. After the reaction was completed, the mixture was filtered, rotary evaporated, and vacuum dried at 60°C for 24 h to obtain a composite sulfide;
[0064] Q2: 1.5 g of hexagonal boron nitride was placed in a mixed solution of 150 mL of isopropanol and 150 mL of deionized water, and then ultrasonically treated for 2 h and then placed in an ultrasonic cleaner for ultrasonic stripping for 12 h. After the stripping was completed, the mixed solution was centrifuged at 5000 rpm for 35 min, vacuum filtered, and vacuum dried at 90 ° C for 12 h to obtain hydroxylated hexagonal boron nitride nanoparticles;
[0065] Q3: 0.2 g of hydroxylated hexagonal boron nitride nanoparticles was added to a mixed solution of 150 mL of ethanol and 50 mL of deionized water, and ultrasonically dispersed for 2 h. Then, 0.5 mL of complex sulfide was added, and the mixture was stirred, condensed and refluxed for 24 h under 100 °C oil bath conditions. The mixture was cooled, filtered, washed and dried to obtain a waterproofing agent.
[0066] Q4: Mix 1kg cement, 2kg sand, 500mL water and 0.15kg waterproofing agent for 12h to obtain waterproof mortar.
[0067] This embodiment discloses a method for preparing a waterproof coating, comprising the following steps:
[0068] S1: Add 8 g of hexachlorocyclotriphosphazene to a container containing 5 mL of chloronaphthalene, heat to 140°C and stir to react, add 0.05 g of palladium after the hexachlorocyclotriphosphazene is completely dissolved, condense and reflux for 10 h, stop heating after the reaction is completed, cool to 100°C, pour the solution into petroleum ether and stir for 3 h to obtain product 1;
[0069] S2: 4.07 mL of hexafluoroisopropanol was added dropwise to 15 mL of tetrahydrofuran containing 1.00 g of metallic sodium using a constant pressure dropping funnel to obtain a mixed solution A; 1.00 g of trifluoroethanol and 8.51 g of octafluoropentanol were added to 15 mL of tetrahydrofuran containing 1.07 g of metallic sodium to obtain a mixed solution B; 5.39 g of the intermediate product 1 was added to 15 mL of tetrahydrofuran containing 1.0 g of metallic sodium using a constant pressure dropping funnel to obtain a mixed solution C;
[0070] S3: Under ice bath conditions, 35 mL of mixed solution A and 115 mL of mixed solution B were added dropwise to 100 mL of mixed solution C. After the addition was completed, the reaction was continued for 12 h. The mixture was first washed with petroleum ether and deionized water in two phases, then washed with deionized water, and dried at 70 °C for 8 h to obtain product 2.
[0071] S4: Add 10 g of product 2 to 30 mL of tetrahydrofuran, stir for 30 min, ultrasonically treat for 45 min, then add 1.0 g of nano-silica particles, and vacuum dry at 70° C. for 4 h to obtain a waterproof coating.
[0072] This embodiment discloses a moisture-proof environmentally friendly construction method for building exterior walls, comprising the following steps:
[0073] Step (1): Clean the surface of the base layer to remove dust, moss and oil stains, and then repair cracks and holes to ensure that the surface of the base layer is flat, clean and free of defects to obtain a building base layer;
[0074] Step (2): using a hot melt method to lay a waterproofing membrane on the surface of a building base layer, and when laying the waterproofing membrane, sealing the end of the membrane to obtain a base layer treated with the waterproofing membrane;
[0075] Step (3): evenly apply the asphalt coating on the surface of the base treated with the waterproof membrane, and then apply the waterproof mortar, apply it multiple times to obtain a building base containing mortar;
[0076] Step (4): After mixing the waterproof coating with water, spray it on the surface of the building base containing mortar, and after drying, paste tiles to obtain a moisture-proof building exterior wall.
[0077] Example 4
[0078] This embodiment discloses a method for preparing a waterproof mortar, comprising the following steps:
[0079] Q1: 2 g of chloropropyltriethoxysilane, 2.5 g of cystamine sulfate, 3.44 g of potassium carbonate, 0.14 g of potassium iodide and 6 mL of anhydrous toluene were added to a dry container, nitrogen was introduced to expel oxygen, and the mixture was heated at 80°C for 24 h under the protection of nitrogen atmosphere. After the reaction was completed, the mixture was filtered, rotary evaporated, and vacuum dried at 60°C for 24 h to obtain a composite sulfide;
[0080] Q2: 2 g of hexagonal boron nitride was placed in a mixed solution of 200 mL of isopropanol and 200 mL of deionized water, and then ultrasonically treated for 2 h and then placed in an ultrasonic cleaner for ultrasonic stripping for 12 h. After the stripping was completed, the mixed solution was centrifuged at 5000 rpm for 35 min, vacuum filtered, and vacuum dried at 90 ° C for 12 h to obtain hydroxylated hexagonal boron nitride nanoparticles;
[0081] Q3: 0.4 g of hydroxylated hexagonal boron nitride nanoparticles was added to a mixed solution of 300 mL of ethanol and 100 mL of deionized water, and ultrasonically dispersed for 2 h. Then 1 mL of complex sulfide was added, and the mixture was stirred, condensed and refluxed for 24 h under 100 °C oil bath conditions. The mixture was cooled, filtered, washed and dried to obtain a waterproofing agent.
[0082] Q4: Mix 3kg cement, 6kg sand, 600mL water and 0.05kg waterproofing agent and stir for 12h to obtain waterproof mortar.
[0083] This embodiment discloses a method for preparing a waterproof coating, comprising the following steps:
[0084] S1: Add 10 g of hexachlorocyclotriphosphazene to a container containing 8 mL of chloronaphthalene, heat to 140°C and stir to react, add 0.08 g of palladium after the hexachlorocyclotriphosphazene is completely dissolved, condense and reflux for 10 h, stop heating after the reaction is completed, cool to 100°C, pour the solution into petroleum ether and stir for 3 h to obtain product 1;
[0085] S2: 5.60 mL of hexafluoroisopropanol was added dropwise to 15 mL of tetrahydrofuran containing 1.33 g of metallic sodium using a constant pressure dropping funnel to obtain a mixed solution A; 1.67 g of trifluoroethanol and 10.05 g of octafluoropentanol were added to 15 mL of tetrahydrofuran containing 1.38 g of metallic sodium to obtain a mixed solution B; 8.99 g of the intermediate product 1 was added to 15 mL of tetrahydrofuran containing 1.67 g of metallic sodium using a constant pressure dropping funnel to obtain a mixed solution C;
[0086] S3: Under ice bath conditions, 70 mL of mixed solution A and 230 mL of mixed solution B were added dropwise to 200 mL of mixed solution C. After the addition was completed, the reaction was continued for 12 h. The mixture was first washed with petroleum ether and deionized water in two phases, then washed with deionized water, and dried at 70 °C for 8 h to obtain product 2.
[0087] S4: Add 20 g of product 2 to 30 mL of tetrahydrofuran, stir for 30 min, ultrasonically treat for 45 min, then add 1.2 g of nano-silica particles, and vacuum dry at 70° C. for 4 h to obtain a waterproof coating.
[0088] This embodiment discloses a moisture-proof environmentally friendly construction method for building exterior walls, comprising the following steps:
[0089] Step (1): Clean the surface of the base layer to remove dust, moss and oil stains, and then repair cracks and holes to ensure that the surface of the base layer is flat, clean and free of defects to obtain a building base layer;
[0090] Step (2): using a hot melt method to lay a waterproofing membrane on the surface of a building base layer, and when laying the waterproofing membrane, sealing the end of the membrane to obtain a base layer treated with the waterproofing membrane;
[0091] Step (3): evenly apply the asphalt coating on the surface of the base treated with the waterproof membrane, and then apply the waterproof mortar, apply it multiple times to obtain a building base containing mortar;
[0092] Step (4): After mixing the waterproof coating with water, spray it on the surface of the building base containing mortar, and after drying, paste tiles to obtain a moisture-proof building exterior wall.
[0093] Example 5
[0094] This embodiment discloses a method for preparing a waterproof mortar, comprising the following steps:
[0095] Q1: 1.7 g of chloropropyltriethoxysilane, 2.07 g of cystamine sulfate, 2.93 g of potassium carbonate, 0.12 g of potassium iodide and 6 mL of anhydrous toluene were added to a dry container, nitrogen was introduced to expel oxygen, and the mixture was heated at 80°C for 24 h under the protection of nitrogen atmosphere. After the reaction was completed, the mixture was filtered, rotary evaporated, and vacuum dried at 60°C for 24 h to obtain a composite sulfide;
[0096] Q2: 1.9 g of hexagonal boron nitride was placed in a mixed solution of 155 mL of isopropanol and 155 mL of deionized water, and ultrasonically treated for 2 h, and then placed in an ultrasonic cleaner for ultrasonic stripping for 12 h. After the stripping, the mixed solution was centrifuged at 5000 rpm for 35 min, vacuum filtered, and vacuum dried at 90 ° C for 12 h to obtain hydroxylated hexagonal boron nitride nanoparticles;
[0097] Q3: 0.35 g of hydroxylated hexagonal boron nitride nanoparticles was added to a mixed solution of 250 mL of ethanol and 60 mL of deionized water, and ultrasonically dispersed for 2 h. Then, 0.6 mL of complex sulfide was added, and the mixture was stirred, condensed and refluxed for 24 h under 100 °C oil bath conditions. The mixture was cooled, filtered, washed and dried to obtain a waterproofing agent.
[0098] Q4: Mix 1.5kg cement, 5kg sand, 540mL water and 0.09kg waterproofing agent and stir for 12h to obtain waterproof mortar.
[0099] This embodiment discloses a method for preparing a waterproof coating, comprising the following steps:
[0100] S1: Add 9.5 g of hexachlorocyclotriphosphazene to a container containing 6.0 mL of chloronaphthalene, heat to 140°C and stir to react, add 0.05 g of palladium after the hexachlorocyclotriphosphazene is completely dissolved, condense and reflux for 10 h, stop heating after the reaction is completed, cool to 100°C, pour the solution into petroleum ether and stir for 3 h to obtain product 1;
[0101] S2: 5.15 mL of hexafluoroisopropanol was added dropwise to 15 mL of tetrahydrofuran containing 1.27 g of metallic sodium using a constant pressure dropping funnel to obtain a mixed solution A; 1.58 g of trifluoroethanol and 9.95 g of octafluoropentanol were added to 15 mL of tetrahydrofuran containing 1.27 g of metallic sodium to obtain a mixed solution B; 8.05 g of the intermediate product 1 was added to 15 mL of tetrahydrofuran containing 1.45 g of metallic sodium using a constant pressure dropping funnel to obtain a mixed solution C;
[0102] S3: Under ice bath conditions, 40 mL of mixed solution A and 128 mL of mixed solution B were added dropwise to 180 mL of mixed solution C. After the addition was completed, the reaction was continued for 12 h. The mixture was first washed with petroleum ether and deionized water in two phases, then washed with deionized water, and dried at 70 °C for 8 h to obtain product 2.
[0103] S4: 18 g of product 2 was added to 30 mL of tetrahydrofuran, stirred for 30 min, ultrasonically treated for 45 min, and then 1.7 g of nano-silica particles was added, and vacuum dried at 70° C. for 4 h to obtain a waterproof coating.
[0104] This embodiment discloses a moisture-proof environmentally friendly construction method for building exterior walls, comprising the following steps:
[0105] Step (1): Clean the surface of the base layer to remove dust, moss and oil stains, and then repair cracks and holes to ensure that the surface of the base layer is flat, clean and free of defects to obtain a building base layer;
[0106] Step (2): using a hot melt method to lay a waterproofing membrane on the surface of a building base layer, and when laying the waterproofing membrane, sealing the end of the membrane to obtain a base layer treated with the waterproofing membrane;
[0107] Step (3): evenly apply the asphalt coating on the surface of the base treated with the waterproof membrane, and then apply the waterproof mortar, apply it multiple times to obtain a building base containing mortar;
[0108] Step (4): After mixing the waterproof coating with water, spray it on the surface of the building base containing mortar, and after drying, paste tiles to obtain a moisture-proof building exterior wall.
[0109] Comparative Example 1
[0110] Compared with Example 2, in Comparative Example 1, during the preparation of the waterproof mortar, no chloropropyltriethoxysilane was added, and other conditions remained unchanged.
[0111] Comparative Example 2
[0112] Compared with Example 2, in Comparative Example 2, no hexagonal boron nitride is added during the preparation of the waterproof mortar, and other conditions remain unchanged.
[0113] Comparative Example 3
[0114] Compared with Example 2, in Comparative Example 3, during the preparation of the waterproof coating, hexachlorocyclotriphosphazene was not added, and other conditions remained unchanged.
[0115] Comparative Example 4
[0116] Compared with Example 2, in Comparative Example 4, hexafluoroisopropanol is not added during the preparation of the waterproof coating, and other conditions remain unchanged.
[0117] Comparative Example 5
[0118] Comparative Example 5 Compared with Example 2, in the process of preparing the waterproof coating in Comparative Example 5, no nano-silica particles are added, and other conditions remain unchanged.
[0119] Comparative Example 6
[0120] Compared with Example 2, in Comparative Example 6, no waterproof mortar is added during the construction of the building exterior wall, and other conditions remain unchanged.
[0121] Comparative Example 7
[0122] Compared with Example 2, in Comparative Example 7, no waterproof coating is added during the construction of the building exterior wall, and other conditions remain unchanged.
[0123] The performance test of the moisture-proof building exterior walls prepared in Examples 2-5 and Comparative Examples 1-7 was carried out to produce a building exterior wall with a volume of 1.00 m×1.00 m×0.30 m, wherein the thickness of the building base layer was 12 cm, the thickness of the waterproof roll material layer was 5.5 cm, the thickness of the waterproof mortar layer was 3 cm, the thickness of the waterproof coating layer was 3 cm, and the thickness of the tile layer was 6.5 cm. The building exterior wall was sprayed with a spray device, the spray flow rate was 18 L / s, the spray time was 30 min, and the weight of the building exterior wall before and after spraying was measured. According to the weight gain rate=[(m 喷淋后 -m 喷淋前 ) / m 喷淋后 ]×100%, the durability of the samples was tested according to GB / T 50082-2009, and the test results are shown in Table 1:
[0124] Table 1
[0125]
[0126]
[0127] It can be seen from the test results in Table 1 that the thermal insulation wall panels prepared in Examples 2-5 of the present invention have excellent moisture-proof performance and durability. The higher the weight gain rate of the building exterior wall, the worse the moisture-proof performance. On the contrary, the lower the weight gain rate of the building exterior wall, the better the moisture-proof performance. By comparing Comparative Example 1 with Examples 2-5, it can be seen that the addition of chloropropyltriethoxysilane can effectively improve the moisture-proof performance and durability of the building's exterior wall; by comparing Comparative Example 2 with Examples 2-5, it can be seen that the addition of hexagonal boron nitride can effectively improve the moisture-proof performance and durability of the building's exterior wall; by comparing Comparative Example 3 with Examples 2-5, it can be seen that the addition of hexachlorocyclotriphosphazene can effectively improve the moisture-proof performance and durability of the building's exterior wall; by comparing Comparative Example 4 with Examples 2-5, it can be seen that the addition of hexafluoroisopropanol can effectively improve the moisture-proof performance of the building's exterior wall; by comparing Comparative Example 5 with Examples 2-5, it can be seen that the addition of nano-silica particles can effectively improve the moisture-proof performance of the building's exterior wall; by comparing Comparative Example 6 with Examples 2-5, it can be seen that the addition of waterproof mortar can effectively improve the moisture-proof performance of the building's exterior wall; by comparing Comparative Example 7 with Examples 2-5, it can be seen that the addition of waterproof coating can effectively improve the moisture-proof performance of the building's exterior wall.
[0128] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0129] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A moisture-proof environmentally friendly construction method for building exterior walls, characterized in that: The following steps are involved: Step (1): Clean the surface of the base layer to remove dust, moss and oil stains, and then repair cracks and holes to ensure that the surface of the base layer is flat, clean and free of defects to obtain a building base layer; Step (2): laying a waterproofing membrane on the surface of a building base using a hot melt method to obtain a base treated with the waterproofing membrane; Step (3): evenly apply the asphalt coating on the surface of the base treated with the waterproof membrane, and then apply the waterproof mortar, apply it multiple times to obtain a building base containing mortar; Step (4): After mixing the waterproof coating with water, spray it on the surface of the building base containing mortar, and after drying, paste tiles to obtain a moisture-proof building exterior wall.
2. A moisture-proof building exterior wall environmental protection construction method according to claim 1, characterized in that: In the step (2), when laying the waterproof coiled material, the end portion of the coiled material is sealed.
3. A moisture-proof building exterior wall environmental protection construction method according to claim 1, characterized in that: In the step (3), the method for preparing the waterproof mortar comprises the following steps: Q1: Add chloropropyltriethoxysilane, cystamine sulfate, potassium carbonate, potassium iodide and anhydrous toluene into a dry container, introduce nitrogen to expel oxygen, heat and react under the protection of nitrogen atmosphere, and after the reaction is completed, filter, rotary evaporate and vacuum dry to obtain a composite sulfide; Q2: placing hexagonal boron nitride in a mixed solution of isopropanol and deionized water, placing it in an ultrasonic cleaner for ultrasonic stripping after ultrasonic treatment, and after the stripping is completed, centrifuging the mixed solution, vacuum filtering, and vacuum drying to obtain hydroxylated hexagonal boron nitride nanoparticles; Q3: Add hydroxylated hexagonal boron nitride nanoparticles to a mixed solution of ethanol and deionized water, disperse by ultrasonication, then add the composite sulfide, stir, condense and reflux under oil bath conditions, cool, filter, wash and dry to obtain a waterproofing agent; Q4: Mix cement, sand, water and waterproofing agent to obtain waterproof mortar.
4. A moisture-proof building exterior wall environmental protection construction method according to claim 3, characterized in that: In the Q1, the molar ratio of chloropropyltriethoxysilane, cystamine sulfate, potassium carbonate and potassium iodide is (0.5-1.0): (0.6-1.2): (1.5-3): (0.05-0.1), the heating reaction temperature is 70-80°C, the heating reaction time is 20-24h, the vacuum drying temperature is 50-60°C, and the time is 20-24h; in the Q2, the amount ratio of hexagonal boron nitride, isopropanol and deionized water is (1.5-2.0)g: (150-200)mL: (150-200)mL, the ultrasonic treatment time is 1-2h, the stripping time is 10-12h, the centrifugal speed is 4000-5000rpm, the centrifugal time is 30-45min, the vacuum drying temperature is 90-110°C, and the time is 10-12h.
5. The moisture-proof environmentally friendly construction method for building exterior walls according to claim 3 is characterized in that: In the Q3, the dosage ratio of hydroxylated hexagonal boron nitride nanoparticles, ethanol, deionized water and complex sulfide is (0.2-0.4) g: (150-300) mL: (50-100) mL: (0.5-1) mL, the ultrasonic dispersion time is 1-2 h, the oil bath temperature is 90-110° C., and the condensation reflux time is 20-24 h. In the Q4, the dosage ratio of cement, sand, water and waterproofing agent is (1-3) kg: (2-6) kg: (500-600) mL: (0.05-0.15) kg, and the mixing and stirring time is 10-12 h.
6. The moisture-proof environmentally friendly construction method for building exterior walls according to claim 1, characterized in that: In the step (4), the method for preparing the waterproof coating comprises the following steps: S1: adding hexachlorocyclotriphosphazene to a container containing chloronaphthalene, heating and stirring to react, adding palladium after the hexachlorocyclotriphosphazene is completely dissolved, condensing and refluxing, stopping heating after the reaction is completed, cooling, and pouring the solution into petroleum ether and stirring to obtain product 1; S2: adding hexafluoroisopropanol to tetrahydrofuran containing metallic sodium using a constant pressure dropping funnel to obtain a mixed solution A; adding trifluoroethanol and octafluoropentanol to tetrahydrofuran containing metallic sodium to obtain a mixed solution B; adding the intermediate product 1 to tetrahydrofuran containing metallic sodium using a constant pressure dropping funnel to obtain a mixed solution C; S3: under ice bath conditions, the mixed solution A and the mixed solution B are added dropwise to the mixed solution C. After the addition is completed, the reaction is continued, and the product 2 is obtained by washing and drying. S4: Add product 2 to tetrahydrofuran, stir, and ultrasonically treat, then add nano-silica particles, and vacuum dry to obtain a waterproof coating.
7. A moisture-proof building exterior wall environmentally friendly construction method according to claim 6, characterized in that: In the S1, the dosage ratio of hexachlorocyclotriphosphazene, chloronaphthalene and palladium is (8-10) g: (5-8) mL: (0.05-0.08) g, the heating temperature is 120-140° C., the condensation reflux time is 8-10 h, the cooling temperature is 90-100° C., and the stirring time is 2-3 h.
8. The moisture-proof environmentally friendly construction method for building exterior walls according to claim 6, characterized in that: In S2, the molar ratio of hexafluoroisopropanol and metallic sodium is (0.8-1.1):(0.9-1.2), the molar ratio of trifluoroethanol, octafluoropentanol and metallic sodium is (0.3-0.5):(1.1-1.3):(1.4-1.8), and the molar ratio of the intermediate product 1 and metallic sodium is (0.3-0.5):(0.3-0.5).
9. The moisture-proof environmentally friendly construction method for building exterior walls according to claim 6, characterized in that: In S3, the volume ratio of mixed solution A, mixed solution B and mixed solution C is (0.35-0.7): (1.15-2.30): (1-2), the reaction time is continued for 10-12 hours, first washed with petroleum ether and deionized water in two phases, and then washed with deionized water, the drying temperature is 60-70°C, and the time is 8-10 hours.
10. The moisture-proof environmentally friendly construction method for building exterior walls according to claim 6, characterized in that: In S4, the mass ratio of product 2 to nano-silicon dioxide particles is (10-20): (1-2), the stirring time is 30-45 min, the ultrasonic treatment time is 30-60 min, the vacuum drying temperature is 60-70° C., and the time is 4-6 h.