Wafer photoresist hardening method and prepared wafer

By performing two-step photoresist treatment and SF6 gas reactive ion etching on the wafer, the limitations of photolithography technology in reducing the key size of semiconductor devices are solved, efficient photoresist hardening is achieved, and the CD size of the wafer is reduced. , reduces production costs and is suitable for large-scale applications.

CN119002181APending Publication Date: 2024-11-22HEFEI IC VALLEY MICROELECTRONICS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411106477.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing lithography technology is limited to the resolution of the lithography machine in reducing the key size of semiconductor devices. The high cost and complex maintenance requirements of high-performance lithography machines hinder further reduction applications. The existing technology is difficult to rely on high performance. In the case of a lithography machine, the CD size of the wafer is effectively controlled and reduced.

Method used

By coating the first photoresist on the wafer and expose and develop, then applying the water-soluble second photoresist and washing and developing, then baking, then performing reactive ion etching using SF6 gas, the line of the photoresist is gradually reduced. Wide, achieve photoresist hardening, avoiding damage to the wafer or harsh performance.

Benefits of technology

The line width value of the wafer CD size measurement is reduced to 0.15~0.3μm. The method is simple and easy to implement and low cost. It is suitable for large-scale promotion and application. It does not require a high-performance lithography machine to meet actual production needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119002181A_ABST
    Figure CN119002181A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of semiconductor manufacturing and processing. The invention provides a photoresist hardening method of a wafer and the prepared wafer, and the method comprises the steps: coating a first photoresist on the wafer, and carrying out the exposure and development to form a first photoresist layer; coating a water-soluble second photoresist on the first photoresist layer, washing with water to obtain a developing effect, and then baking; and performing reactive ion etching by using SF6 gas to harden the photoresist. According to the method, the formed first photoresist layer is subjected to two-step treatment, the line width is gradually reduced, dependence on a high-performance photoetching machine is not needed, namely, the CD size measurement line width value of the wafer is reduced to 0.15-0.3 mu m, and the method is simple, easy to implement, low in cost and beneficial to large-scale popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor manufacturing and processing, and relates to a photoresist hardening method for a wafer and the prepared wafer. Background Art

[0002] With the rapid development of semiconductor technology, gallium arsenide (GaAs) wafers have shown great application potential in the fields of high-frequency, high-speed, high-power electronic devices and optoelectronic devices due to their superior electron mobility and direct bandgap characteristics. In the micro-nano manufacturing process of GaAs-based devices, photolithography technology is the core step to achieve the refinement of circuit patterns, and its accuracy and efficiency directly affect the performance and cost of the device. Among them, photoresist is the key material for carrying pattern transfer, and its performance optimization and processing technology control play a decisive role in reducing the critical dimension (CD size) of the device.

[0003] The photolithography process mainly includes the steps of coating photoresist, exposure, development, etching, etc. First, the photosensitive material photoresist (photoresist) is evenly coated on the surface of the wafer to form a thin film. Subsequently, a photolithography machine is used to project light of a specific pattern. Through the sensitivity of the photoresist to light of a specific wavelength, the photoresist in the light-irradiated area or the unirradiated area undergoes chemical changes. This process is called exposure. Next, the exposed or unexposed part of the photoresist is removed by a developer, leaving the desired circuit pattern on the wafer. Finally, the pattern is used as a mask for etching or other subsequent processing to transfer the circuit pattern to the wafer substrate material.

[0004] Photoresist hardening is an indispensable part of the photolithography process, which aims to improve the etching resistance and thermal stability of the photoresist, and ensure that the photoresist pattern can maintain a good shape and avoid deformation or dissolution under the harsh conditions of subsequent etching, ion implantation, etc., so as to ensure the accuracy and reliability of the final device. Through hardening treatment, the physical properties of the photoresist are significantly improved, and it can withstand more complex manufacturing processes, which is crucial to achieving smaller critical dimensions.

[0005] At present, as semiconductor devices advance to a higher level of integration, reducing critical dimensions has become the key to improving performance and reducing energy consumption. However, this process is strictly limited by the resolution of lithography machines. Although current mainstream lithography technologies, such as deep ultraviolet (DUV) and extreme ultraviolet (EUV) lithography, continue to push the limits of resolution, the high cost, complex system maintenance, and stringent requirements for materials and processes make it particularly important to find solutions and means that do not rely entirely on high-performance lithography machines to further reduce critical dimensions.

[0006] Faced with the above challenges, researchers have explored a variety of strategies to circumvent the direct limitations of lithography machine resolution, including but not limited to self-assembly technology, nanoimprint lithography (NIL), electron beam lithography (EBL) and directed self-assembly (DSA). These technologies have their own characteristics, but they also face different limitations. Self-assembly technology is limited by the complexity and controllability of the pattern; nanoimprint lithography has mold durability and cost issues in large-scale production; electron beam lithography is difficult to apply to large-scale production due to its slow processing speed and high equipment cost; directed self-assembly technology still has challenges in realizing complex three-dimensional structures, and has strict requirements on materials and environmental conditions. The above limiting factors have, to a certain extent, hindered the widespread application of these technologies in actual production.

[0007] In view of this, changing the thinking to optimize and improve the photoresist hardening method is an important research direction with high value and high application potential, aiming to effectively control and further reduce the critical dimensions without relying on high-performance lithography machines and other related equipment. Summary of the invention

[0008] In view of the problems existing in the prior art, the purpose of the present invention is to provide a photoresist hardening method for a wafer and a wafer obtained, the method comprising coating a first photoresist on the wafer, exposing and developing to form a first photoresist layer; coating a water-soluble second photoresist on the first photoresist layer, washing with water to obtain a developing effect and then baking; and then using SF6 gas for reactive ion etching to harden the photoresist. The present invention gradually reduces the line width by performing two-step processing on the formed first photoresist layer, and does not need to rely on a high-performance lithography machine, that is, the CD size measurement line width value of the wafer is reduced to 0.15-0.3μm. The method is simple and easy to implement and has low cost, which is conducive to large-scale promotion and application.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a method for curing photoresist of a wafer, comprising:

[0011] (1) coating a first photoresist on the wafer, and developing after exposure to form a first photoresist layer;

[0012] (2) coating a water-soluble second photoresist on the first photoresist layer, washing, developing, and then baking;

[0013] (3) Use SF6 gas for reactive ion etching to harden the photoresist.

[0014] The present invention obtains a developing effect by coating a first photoresist and performing conventional exposure and development, and then coating a water-soluble second photoresist and washing with water. Since the second photoresist is soluble in water, the developing effect can be achieved by controlling the washing time, that is, the ideal CD size can be further reduced. On this basis, the present invention innovatively proposes to use SF6 gas for reactive ion etching to process the photoresist to further reduce the CD size of the wafer, and this method will not cause damage to the wafer or have other adverse effects on the product structure and performance. The present invention gradually reduces the line width by performing two-step processing on the formed first photoresist layer, and does not need to rely on a high-performance lithography machine, that is, the CD size measurement line width value of the wafer is reduced to 0.15-0.3μm. The method is simple and easy to implement and has low cost, can be implemented by commonly used semiconductor equipment, does not need to purchase additional equipment to save costs, meets actual production needs, and is conducive to large-scale promotion and application.

[0015] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0016] As a preferred technical solution of the present invention, in step (1), the wafer includes a gallium arsenide wafer.

[0017] Preferably, the wafer is cleaned before coating the first photoresist.

[0018] Preferably, the method for cleaning the wafer comprises alkaline washing followed by spin drying.

[0019] Preferably, the alkaline solution for alkali washing comprises aqueous ammonia.

[0020] Preferably, the alkali washing time is 5 to 8 minutes, for example, 5 minutes, 6 minutes, 7 minutes or 8 minutes.

[0021] Preferably, the spin-drying time is 20 to 40 minutes, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes.

[0022] As a preferred technical solution of the present invention, in step (1), the first photoresist includes AR80.

[0023] Preferably, the thickness of the first photoresist layer is For example or etc., preferably More preferably

[0024] Too small or too large coating thickness of the first photoresist will affect the CD size of the first photoresist layer. Since it is a basic size, the coating thickness and the thickness of the first photoresist layer should be reasonably adjusted according to actual needs to prevent the CD size from being too large or too small, thereby affecting the subsequent further reduction of the line width after the photoresist is hardened.

[0025] As a preferred technical solution of the present invention, in step (1), after the first photoresist layer is formed, the CD size measurement line width value of the obtained first photoresist layer is 0.41-0.51 μm, for example, 0.41 μm, 0.42 μm, 0.43 μm, 0.44 μm, 0.45 μm, 0.46 μm, 0.47 μm, 0.48 μm, 0.49 μm, 0.50 μm or 0.51 μm, etc., preferably 0.41-0.48 μm, and more preferably 0.41-0.44 μm.

[0026] As a preferred technical solution of the present invention, in step (2), the water-soluble second photoresist includes R200.

[0027] Preferably, the coating thickness of the water-soluble second photoresist is For example or etc., preferably More preferably

[0028] Too small or too large a coating thickness of the second photoresist may also cause the CD size of the second photoresist layer to be too large or too small, thereby affecting the further reduction of the line width after subsequent photoresist hardening.

[0029] Preferably, the water washing and development is performed using deionized water.

[0030] Preferably, the time for the water washing and developing is 22 to 38 s, for example, 22 s, 24 s, 26 s, 28 s, 30 s, 32 s, 34 s, 36 s or 38 s.

[0031] As a preferred technical solution of the present invention, in step (2), a water-soluble second photoresist is coated, and after water washing and development, before baking, the CD size measurement line width value of the formed second photoresist layer is 0.27 to 0.37 μm, for example, 0.27 μm, 0.28 μm, 0.29 μm, 0.3 μm, 0.31 μm, 0.32 μm, 0.33 μm, 0.34 μm, 0.35 μm, 0.36 μm or 0.37 μm, etc., preferably 0.27 to 0.34 μm, and more preferably 0.27 to 0.3 μm.

[0032] Preferably, the baking temperature is 110-140°C, for example 110°C, 115°C, 120°C, 125°C, 130°C, 135°C or 140°C, etc., preferably 121-127°C; the baking time is 30-50min, for example 30min, 35min, 40min, 45min or 50min, etc., preferably 42-48min.

[0033] In the present invention, it is preferred to bake in a dust-free and oxygen-free vacuum oven. The purpose of baking is to evaporate the water content of the photoresist so that the pattern can be further fixed. When the baking temperature is too low, the water content of the photoresist will not evaporate sufficiently, affecting the subsequent process. When the baking temperature is too high, the photoresist may become sticky, directly causing the wafer to be scrapped.

[0034] As a preferred technical solution of the present invention, in step (3), the flow rate of the SF6 gas is 80-120 sccm, for example, 80 sccm, 85 sccm, 90 sccm, 95 sccm, 100 sccm, 105 sccm, 110 sccm, 115 sccm or 120 sccm, etc., preferably 90-110 sccm, and more preferably 98-102 sccm.

[0035] As a preferred technical solution of the present invention, in step (3), the radio frequency of the reactive ion etching includes RF radio frequency.

[0036] Preferably, the RF power of the reactive ion etching is 50-80W, for example, 50W, 55W, 60W, 65W, 70W, 75W or 80W, etc., preferably 56-74W, and more preferably 62-68W.

[0037] Preferably, the chamber pressure of the reactive ion etching is 110-140 mTorr, for example, 110 mTorr, 115 mTorr, 120 mTorr, 125 mTorr, 130 mTorr, 135 mTorr or 140 mTorr, etc., preferably 117-133 mTorr, and more preferably 123-127 mTorr.

[0038] Preferably, the chamber temperature of the reactive ion etching is 110-140° C., for example, 110° C., 115° C., 120° C., 125° C., 130° C., 135° C. or 140° C.

[0039] Preferably, the reactive ion etching time is 42 to 48 s, for example, 42 s, 43 s, 44 s, 45 s, 46 s, 47 s or 48 s.

[0040] As a preferred technical solution of the present invention, in step (3), after the photoresist is hardened, the CD size measurement line width value of the wafer is 0.2-0.3μm, for example, 0.2μm, 0.21μm, 0.22μm, 0.23μm, 0.24μm, 0.25μm, 0.26μm, 0.27μm, 0.28μm, 0.29μm or 0.3μm, etc., preferably 0.2-0.27μm, and more preferably 0.2-0.22μm.

[0041] In step (3) of the present invention, the necessary conditions for the machine for performing reactive ion etching during the photoresist hardening include changes in RF power, gas flow, chamber pressure, chamber temperature, and reactive ion etching time, which will affect whether the CD size is too high or too low. The parameters should be reasonably selected and adjusted to obtain the best effect of reducing the CD size.

[0042] In a second aspect, the present invention provides a photoresist-hardened wafer obtained according to the photoresist-hardening method described in the first aspect.

[0043] Due to space limitations and to avoid redundancy, the present invention does not list all point values ​​within the above numerical range one by one, but is not limited to the listed values, and other unlisted values ​​within the above numerical range are also applicable.

[0044] Compared with the prior art solutions, the present invention has at least the following beneficial effects:

[0045] The method for photoresist hardening of the wafer of the present invention performs two-step processing on the formed first photoresist layer to gradually reduce the line width without relying on a high-performance lithography machine, that is, the CD size measurement line width value of the wafer is reduced to 0.15-0.3 μm. The method is simple and easy and has low cost. It can be implemented by common semiconductor equipment, does not require additional equipment to save cost, meets actual production needs, and is conducive to large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 Schematic diagram of the CD line width change of the wafer in the photoresist hardening method in Example 1. DETAILED DESCRIPTION

[0047] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0048] It should be clear to those skilled in the art that the embodiments are only intended to help understand the present invention and should not be considered as specific limitations of the present invention.

[0049] Example 1

[0050] This embodiment provides a method for curing photoresist of a wafer. Figure 1As shown, the photoresist hardening method includes:

[0051] (1) The gallium arsenide wafer was cleaned for 6 minutes using an alkaline solution (composed of 30% ammonia water and deionized water in a mass ratio of 1:50) in a tank cleaning machine, and then dried in a horizontal spin dryer for 30 minutes; a first layer of photoresist (AR80) was coated on the cleaned wafer using a photoresist coater, and after exposure and development by a photolithography machine, a layer of photoresist with a thickness of 10000 was formed. The first photoresist layer; after testing, the CD size of the first photoresist layer ( Figure 1 A) The measured line width is 0.45-0.47 μm;

[0052] (2) coating a water-soluble second photoresist (R200) ​​on the first photoresist layer, and controlling the coating thickness to Deionized water was used to clean and develop for 30 seconds. After testing, the CD size of the second photoresist layer formed at this time ( Figure 1 B) The measured line width is 0.31-0.33 μm. The wafer is placed in a vacuum oven and baked at 124°C for 45 minutes.

[0053] (3) The baked GaAs wafer is placed in an RIE etcher, and the GaAs wafer and the sapphire carrier are bonded in a vacuum chamber. The pressing force is 650N. SF6 is used for RIE (reactive ion etching). The RF power is controlled to be 65W, the process chamber pressure is maintained at 125mT, the SF6 flow rate is 100sccm, and the etching photoresist hardening time is 45s. After testing, the CD size of the wafer ( Figure 1 The measured line width value of C) is 0.15-0.26 μm.

[0054] The equipment used in the photoresist hardening method of the wafer described in this embodiment includes: a tank cleaning machine, a photoresist coater, a photolithography machine, a RIE etcher, a vacuum oven, etc. Precautions are as follows: ① The RIE etcher uses toxic and harmful gases, and the gas closed loop state of the equipment needs to be confirmed before using the equipment; ② The RIE dry etcher is a high vacuum equipment, and the process is not allowed to proceed before the vacuum pressure reaches the process use requirements; ③ The tank cleaning machine, the photoresist coater, and the vacuum oven use chemicals and high temperature environments during production operations, and personnel need to take protective measures.

[0055] Example 2

[0056] This embodiment provides a method for hardening photoresist of a wafer. In step (2) of the method for hardening photoresist, the baking temperature is adjusted from 124° C. to 100° C. Except for the above, other conditions are exactly the same as those in Example 1.

[0057] Example 3

[0058] This embodiment provides a method for photoresist hardening of a wafer. In step (2) of the photoresist hardening method, the baking temperature is adjusted from 124° C. to 110° C. Except for the above, other conditions are exactly the same as those in Example 1.

[0059] Example 4

[0060] This embodiment provides a photoresist hardening method for a wafer. In step (3) of the photoresist hardening method, the flow rate of SF6 is adjusted from 100 sccm to 80 sccm. Except for the above, other conditions are exactly the same as those in Example 1.

[0061] Example 5

[0062] This embodiment provides a method for photoresist hardening of wafers. In step (3) of the photoresist hardening method, the flow rate of SF6 is adjusted from 100 sccm to 120 sccm. Except for the above, other conditions are exactly the same as those in Example 1.

[0063] Comparative Example 1

[0064] This comparative example provides a method for photoresist hardening of a wafer, wherein the photoresist hardening method does not perform step (2) but only performs step (1) and step (3). Except for the above, other conditions are exactly the same as those in Example 1.

[0065] Table 1

[0066]

[0067]

[0068] It can be seen from Table 1 that:

[0069] In the present invention, the first photoresist coated in step (1) must have an appropriate thickness. Otherwise, coating too low or too late will cause the morphology to change, making it impossible to measure. When the first photoresist layer has a clear basic CD size as a basis, the line width can be effectively reduced through steps (2) and (3).

[0070] When the baking temperature in step (2) is too low, insufficient evaporation of the water in the photoresist will result in unsatisfactory line width reduction. When the baking temperature in step (2) is too high, the photoresist will become sticky, resulting in the wafer being scrapped.

[0071] Step (3) If the SF6 gas flow rate in the cavity is too high or too low, it will lead to failure of ignition and hardening. Moreover, ignition and hardening within a certain range will also lead to large errors in the measurement data.

[0072] From the above, it can be seen that the photoresist hardening method for wafers provided by the present invention can realize the optimized photoresist hardening of GaAs wafers (devices) to control and reduce the line width, and can achieve a small line width level without the need for a high-performance lithography machine, thereby improving product performance; the newly added process steps can all be implemented through commonly used semiconductor equipment, and there is no need to purchase additional equipment to save costs, which meets actual production needs.

[0073] The present invention uses the above-mentioned embodiments to illustrate the details and process flow of the present invention, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0074] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0075] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0076] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for curing photoresist of a wafer, characterized in that: include: (1) coating a first photoresist on the wafer, and developing after exposure to form a first photoresist layer; (2) coating a water-soluble second photoresist on the first photoresist layer, washing, developing, and then baking; (3) Use SF6 gas for reactive ion etching to harden the photoresist.

2. The method for curing photoresist of a wafer according to claim 1, characterized in that: In step (1), the wafer comprises a gallium arsenide wafer; Preferably, the wafer is cleaned before coating the first photoresist; Preferably, the method for cleaning the wafer comprises alkali washing followed by spin drying; Preferably, the alkaline liquid for alkali washing comprises aqueous ammonia; Preferably, the alkali washing time is 5 to 8 minutes; Preferably, the spin-drying time is 20 to 40 minutes.

3. The method for curing photoresist of a wafer according to claim 1 or 2, characterized in that: In step (1), the first photoresist comprises AR80; Preferably, the thickness of the first photoresist layer is 4. The method for curing photoresist of a wafer according to any one of claims 1 to 3, characterized in that: In step (1), after forming the first photoresist layer, the CD dimension measurement line width value of the obtained first photoresist layer is 0.41-0.51 μm.

5. The method for curing photoresist of a wafer according to any one of claims 1 to 4, characterized in that: In step (2), the water-soluble second photoresist includes R200; Preferably, the coating thickness of the water-soluble second photoresist is Preferably, the water washing and development is carried out using deionized water; Preferably, the time of the water washing and developing is 22 to 38 seconds.

6. The method for curing photoresist of a wafer according to any one of claims 1 to 5, characterized in that: In step (2), a water-soluble second photoresist is coated, and after washing and development, and before baking, the CD dimension measurement line width value of the formed second photoresist layer is 0.27 to 0.37 μm; Preferably, the baking temperature is 110-140° C. and the baking time is 30-50 min.

7. The method for curing photoresist of a wafer according to any one of claims 1 to 6, characterized in that: In step (3), the flow rate of the SF6 gas is 80 to 120 sccm.

8. The method for curing photoresist of a wafer according to any one of claims 1 to 7, characterized in that: In step (3), the radio frequency of the reactive ion etching includes RF radio frequency; Preferably, the radio frequency power of the reactive ion etching is 50 to 80 W; Preferably, the chamber pressure of the reactive ion etching is 110-140 mTorr; Preferably, the chamber temperature of the reactive ion etching is 110-140°C; Preferably, the reactive ion etching time is 42 to 48 seconds.

9. The method for curing photoresist of a wafer according to any one of claims 1 to 8, characterized in that: In step (3), after the photoresist is hardened, the line width of the wafer is measured by CD dimension at 0.2-0.3 μm.

10. A photoresist-hardened wafer, characterized in that: Obtained according to the photoresist hardening method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Electrode manufacturing method of mesa detector and mesa detector

    CN121531814A