Preparation method of multi-layer conductive structure, conductive structure and electronic device
By preparing conductive holes and metal pattern layers on the silk fibroin membrane and bonding according to preset structural levels, the problems of biocompatibility and degradability of traditional conductive materials in biomedical and wearable devices are solved, and the problem of biocompatibility and degradability of traditional conductive materials in biomedical and wearable devices is achieved. High-performance multi-layer conductive structure.
Patent Information
- Application Number
- CN202411031444.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Traditional conductive materials lack biocompatibility and degradability in electronic devices, making them difficult to apply in biomedical and wearable devices. In particular, there are technical challenges in preparing silk fibroin-based multilayer structures with excellent conductive functions.
By providing at least two silk fibroin membranes, conductive holes and metal pattern layers are prepared on each membrane, and bonded according to preset structural levels to form a multi-layer conductive structure, and the conductive holes are filled with silk fibroin and carbon nanotubes. The aqueous solution was dried and the metal pattern layer was prepared by electron beam evaporation or screen printing technology.
While maintaining biocompatibility and mechanical properties, it is achieved to prepare conductive structures with better biocompatibility, mechanical properties and degradability, suitable for biomedical and wearable devices.
Smart Images

Figure CN119008113A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of microelectronic technology, and in particular to a method for preparing a multi-layer conductive structure, a conductive structure and an electronic device. Background Art
[0002] With the continuous progress of materials science, microelectronics and micro-nano processing technology, the demand for higher performance, smaller, safer, and more environmentally sustainable electronic products is growing. Especially in the field of biomedical and wearable devices, the demand for materials with good compatibility with the human body, excellent mechanical properties and environmental friendliness is particularly urgent.
[0003] Although traditional conductive materials such as metals and synthetic polymers are widely used in electronic devices, they often lack sufficient biocompatibility and degradability, and have limitations in their application in flexible and wearable devices. Silk fibroin, as a natural protein, is considered an ideal candidate material to solve the above problems due to its excellent biocompatibility, excellent mechanical strength and biodegradability.
[0004] However, how to realize the application of silk fibroin in the electronic field while maintaining its biocompatibility and mechanical properties, especially how to prepare silk fibroin-based multilayer structures with excellent conductive functions, remains a technical challenge. Summary of the invention
[0005] In order to solve the above technical problems, the present application discloses, on one hand, a method for preparing a multilayer conductive structure, which comprises:
[0006] providing at least two silk fibroin films;
[0007] Preparing conductive holes and a metal pattern layer on each of the at least two silk fibroin films to obtain at least two target silk fibroin films;
[0008] Bonding the at least two target silk fibroin films according to a preset structural hierarchy to form a multi-layer conductive structure;
[0009] Wherein, preparing conductive holes on each of the silk fibroin membranes comprises:
[0010] forming a preset through hole on the silk fibroin film;
[0011] Filling the preset through hole with conductive ink; the conductive ink is an aqueous solution of a polymer formed by silk fibroin and carbon nanotubes;
[0012] Then, a first drying process is performed to form the conductive hole.
[0013] Furthermore, forming a preset through hole on the silk fibroin film comprises:
[0014] Two blocking members are provided;
[0015] Placing a blocking member on the upper and lower surfaces of the silk fibroin film respectively to form an intermediate structure; the size of the blocking member is greater than or equal to the size of the silk fibroin film;
[0016] A laser punching process is used to form a preset through hole on the intermediate structure.
[0017] Furthermore, the conditions of the first drying process include:
[0018] The drying temperature is 40-50°C and the drying time is 1-3 hours.
[0019] Furthermore, the diameter of the preset through hole is 0.05-0.2 mm;
[0020] The material of the barrier member includes polyvinyl alcohol.
[0021] Further, a metal pattern layer is prepared on each of the silk fibroin films, comprising:
[0022] forming a mask pattern on the silk fibroin film;
[0023] The metal pattern layer is formed by evaporating the metal onto the silk fibroin film through the mask pattern using electron beam evaporation technology, and the mask pattern is removed.
[0024] Further, a metal pattern layer is prepared on each of the silk fibroin films, comprising:
[0025] Using screen printing technology to scrape the conductive ink onto the silk fibroin film;
[0026] A second drying process is then performed to form the metal pattern layer.
[0027] Furthermore, the step of bonding the at least two target silk fibroin films according to a preset structural hierarchy to form a multilayer conductive structure includes:
[0028] performing plasma cleaning treatment on at least two of the target silk fibroin films respectively;
[0029] Coating the silk fibroin solution on the surfaces to be bonded in at least two of the target silk fibroin films respectively;
[0030] stacking and pressing at least two of the target silk fibroin films according to a preset structural hierarchy to obtain an initial multi-layer conductive structure;
[0031] The initial multi-layer conductive structure is subjected to steam cross-linking and drying treatments in sequence to obtain the multi-layer conductive structure.
[0032] Furthermore, the step of preparing conductive holes and a metal pattern layer on each of the at least two silk fibroin films to obtain at least two target silk fibroin films comprises:
[0033] Conductive holes are prepared on each of the at least two silk fibroin membranes, and a metal pattern layer is prepared on each of the silk fibroin membranes to obtain at least two target silk fibroin membranes; or a metal pattern layer is prepared on each of the at least two silk fibroin membranes, and a conductive hole is prepared on each of the silk fibroin membranes to obtain at least two target silk fibroin membranes.
[0034] On the other hand, the present application further discloses a conductive structure, which is prepared using the above-mentioned preparation method.
[0035] In another aspect, the present application further discloses an electronic device, which includes the above-mentioned conductive structure.
[0036] The embodiment of the present application provides a method for preparing a multilayer conductive structure, by providing at least two silk fibroin films; preparing conductive holes and a metal pattern layer on each of the at least two silk fibroin films to obtain at least two target silk fibroin films; bonding the at least two target silk fibroin films according to a preset structural hierarchy to form a multilayer conductive structure; wherein the conductive holes are prepared on each of the silk fibroin films by forming a preset through hole on the silk fibroin film; filling the preset through hole with conductive ink; the conductive ink is an aqueous solution of a polymer formed by silk fibroin and carbon nanotubes; and then performing a first drying process to form the conductive holes. In this way, the entire molding process is not only simple, but also the conductive structure formed has better biocompatibility, mechanical properties and degradability. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0038] Figure 1 A schematic diagram of a process for preparing a multi-layer conductive structure exemplified in the present application;
[0039] Figure 2 This is a schematic diagram of the structure of a silk fibroin membrane with preset through holes exemplified in the present application;
[0040] Figure 3 This is a schematic diagram of the structure of a silk fibroin membrane with conductive holes exemplified in the present application;
[0041] Figure 4 This is a schematic diagram of the structure of an exemplary target silk fibroin membrane of the present application.
[0042] The following is a supplementary description of the attached drawings:
[0043] 1-silk fibroin film; 11-first silk fibroin film; 12-second silk fibroin film; 2-preset through hole; 3-conductive hole; 4-metal graphic layer. DETAILED DESCRIPTION
[0044] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0045] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure or characteristic that may be included in at least one implementation of the present application. In the description of the present application, it should be understood that the orientation or positional relationship indicated by the terms "upper", "lower", "top", "bottom", etc. is based on the orientation or positional relationship shown in the accompanying drawings, which is only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present application. In addition, the terms "first" and "second" are used only for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may include one or more of the features explicitly or implicitly. Moreover, the terms "first", "second", etc. are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present application described here can be implemented in an order other than those illustrated or described here.
[0046] For the purpose of the following detailed description, it should be understood that the present invention may adopt various alternative changes and step sequences, unless expressly specified to the contrary. In addition, except in any operating examples, or otherwise indicated, all numbers representing the amount of ingredients used in the specification and claims should be understood to be modified by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters set forth in the following specification and the attached claims are approximate values that vary according to the desired performance to be obtained by the present invention. At least it is not intended to limit the application of the doctrine of equivalents to the scope of the claims, and each numerical parameter should at least be interpreted according to the number of reported significant figures and by applying ordinary rounding techniques.
[0047] Notwithstanding that the numerical ranges and parameters setting forth the broad scope of the invention are approximations, the numerical values set forth in the specific examples are reported as precisely as possible. Any numerical value, however, inherently contains certain errors necessarily resulting from the standard deviation found in their respective testing measurements.
[0048] When a numerical range is disclosed herein, the above range is deemed to be continuous and includes the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all sub-ranges included therein. For example, a specified range from "1 to 10" should be deemed to include any and all sub-ranges between a minimum of 1 and a maximum of 10. Exemplary sub-ranges of ranges 1 to 10 include, but are not limited to, 1 to 6.1, 3.5 to 7.8, 5.5 to 10, etc.
[0049] See also Figure 1 , which is a schematic flow chart of a method for preparing a multi-layer conductive structure exemplified in the present application. The method for preparing the multi-layer conductive structure may specifically include:
[0050] S101: providing at least two silk fibroin films.
[0051] In the embodiment of the present application, the silk fibroin film 1 can be obtained directly, or it can be prepared by the following method: first preparing a silk fibroin aqueous solution, forming a silk fibroin wet film based on the silk fibroin aqueous solution, and then placing the silk fibroin wet film in a vacuum water vapor environment to cross-link the silk fibroin molecules of the silk fibroin wet film to form the silk fibroin film 1.
[0052] The silk fibroin aqueous solution can be prepared by the following steps:
[0053] 1) Weighing dry and clean silk cocoons, placing them in a sodium carbonate solution, and performing a heating treatment to remove sericin from the cocoons, thereby completing degumming and forming silk.
[0054] For example, the silk cocoons can be cut into pieces and placed in a sodium carbonate solution, and then heated and stirred. The silk cocoons are silk cocoons after the pupae are removed.
[0055] An exemplary concentration of the sodium carbonate solution is 0.1-3 g / L, and the volume ratio of the mass of the silk cocoon to the sodium carbonate solution is (5:2), in units of g / L.
[0056] An exemplary heating method of the sodium carbonate solution may be electric furnace heating or pressure cooker heating, with a heating temperature of 60 to 100° C., a heating pressure of 0.5 to 1 MPa, and a heating time of 1 second to 1000 hours.
[0057] 2) placing the silk in deionized water and washing it multiple times.
[0058] An exemplary method of washing the silk is stirring washing or static soaking, wherein the stirring method of stirring washing is mechanical stirring or magnetic stirring, and the magnetic stirring speed is 1 to 2000 r / min; during a single washing process, the mass ratio of the silk to the ultrapure water is 1:20 to 1:50, the unit is g / L, and the time is 60s to 5h; after each washing, the silk is taken out and squeezed dry, and the washing is repeated 1 to 50 times.
[0059] 3) Drying the washed silk, stirring and mixing the dried silk with the lithium salt aqueous solution, and keeping the mixture warm for a period of time to obtain the silk fibroin lithium salt aqueous solution.
[0060] An exemplary drying treatment method is natural air drying or heated ventilation drying, wherein the temperature of the heated ventilation drying is 50 to 70° C. and the drying time is 1 to 20 hours.
[0061] An exemplary lithium salt aqueous solution is a lithium thiocyanate solution or a lithium bromide solution, the concentration of the lithium salt aqueous solution is 0.01 to 2 g / ml, the volume ratio of the mass of the dried silk to the lithium salt aqueous solution is (1 to 100): 100, g / ml; the insulation temperature is 30 to 80°C, and the insulation time is 0.5 to 5h.
[0062] The use of lithium salt aqueous solution can break the hydrogen bond network within silk fibers, thereby dissolving the silk fibroin into a silk fibroin solution to generate new materials.
[0063] 4) Pour the silk fibroin lithium salt aqueous solution into a dialysis bag and dialyze it in ultrapure water.
[0064] Exemplarily, the dialysis method is static dialysis or magnetic stirring dialysis. Optionally, the specification of the dialysis bag is 10-1000000Da, and the dialysis method is static dialysis or magnetic stirring dialysis; the stirring speed of the magnetic stirring dialysis is 1-2000r / min, the time interval for changing water during the dialysis process is 0.1-100h, and the volume of ultrapure water required for each dialysis is 1mL-1000L. After dialysis, the dissolved lithium bromide can be removed to prevent subsequent ion residues from causing harm to people.
[0065] Exemplarily, the stirring speed is 60 to 300 r / min, and the time interval for changing water during the dialysis process is 1 to 24 hours.
[0066] 5) Centrifuging the dialyzed silk fibroin lithium salt aqueous solution, collecting the supernatant after centrifugation, and obtaining the silk fibroin aqueous solution.
[0067] Exemplarily, the rotation speed of the centrifugal treatment is 10 to 20,000 r / min, the time is 6 s to 2 h, and the temperature is -3 to 5° C. The concentration of the silk fibroin aqueous solution 1 is 0.05 to 0.25 g / ml.
[0068] The method for forming a silk fibroin wet film comprises: coating the silk fibroin aqueous solution on a flat mold, and standing under preset temperature and humidity conditions to form the silk fibroin wet film. Optionally, the silk fibroin aqueous solution can be transferred by a pipette and injected into the flat mold, then the silk fibroin aqueous solution is scraped evenly to make the solution thickness reach a preset thickness, and the small bubbles on the surface of the solution are sucked away with a dropper, and the plate covered with the silk fibroin aqueous solution is naturally dried under preset temperature and humidity conditions to form a film. Optionally, the volume of the pipette is 0.1 to 20 ml; the area of the flat mold is 0.01 to 100 cm2.
[0069] Exemplarily, the preset temperature and humidity conditions include: a temperature range of 15 to 25° C.; a humidity range of 38 to 39% RH; and a standing time of 1 to 100 hours.
[0070] Exemplarily, the thickness of the silk fibroin aqueous solution coated on the flat mold ranges from 0.1 to 10 mm.
[0071] Exemplarily, the flat plate mold may be one or a combination of acrylic plate, polystyrene plate, polypropylene plate and metal plate.
[0072] Subsequently, it is necessary to cut off the uneven edges of the silk fibroin wet film and then place it on a flat mold.
[0073] The wet silk fibroin film is placed in a vacuum water vapor environment to cross-link the silk fibroin molecules of the wet silk fibroin film to form the silk fibroin film 1. The specific implementation method may include: placing the wet silk fibroin film in a vacuum kettle containing water, and opening the vacuum kettle; the air pressure of the vacuum kettle is -0.01 to -0.1 MPa. Optionally, the wet silk fibroin film is placed in the vacuum kettle 4 for cross-linking for 1 to 50 hours, and the insoluble silk fibroin film 1 can be obtained after the cross-linking is completed.
[0074] S103: preparing conductive holes and a metal pattern layer on each of the at least two silk fibroin films to obtain at least two target silk fibroin films.
[0075] In the embodiment of the present application, the target silk protein film 1 can be specifically as follows Figure 3 The structure of the two silk fibroin films 1 shown in the figure, assuming that the embodiment of the present application provides two silk fibroin films 1 in step S101, which are respectively called the first silk fibroin film 11 and the second silk fibroin film 12, by sequentially preparing the conductive holes 3 and the metal pattern layer 4 in the first silk fibroin film 11 and the second silk fibroin film 12, respectively, the following can be obtained: Figure 3 In order to realize the electrical connection of the metal pattern layers 4 on the two target silk fibroin films 1, the positions of the conductive holes 3 on the two silk fibroin films 1 should correspond to each other to form a conductive path. Specifically, the target silk fibroin film 1 corresponding to the first silk fibroin film 11 can be used as the bottom layer, and the second silk fibroin film 12 can be used as the top layer. Then, after the subsequent stacking is completed, the second silk fibroin film 12 is located on the first silk fibroin film 11.
[0076] In a feasible embodiment, step S102 may specifically include: preparing a conductive hole 3 on each of the at least two silk fibroin films 1 to obtain a conductive hole 3. Figure 4 The structure shown in FIG. 1 is further provided, and a metal graphic layer 4 is prepared on each of the silk fibroin films 1 to obtain at least two target silk fibroin films 1, that is, a conductive hole 3 can be formed on the silk fibroin film 1 first, and then a metal graphic layer 4 is formed. In another feasible embodiment, step S102 can specifically include preparing a metal graphic layer 4 on each of the at least two silk fibroin films 1, and then preparing a conductive hole 3 on each of the silk fibroin films 1 to obtain at least two target silk fibroin films 1. That is, a metal graphic layer 4 can be formed on the silk fibroin film 1 first, and then a conductive hole 3 can be formed. No limitation is made here.
[0077] Wherein, preparing the conductive hole 3 on each of the silk fibroin membranes 1 comprises: forming a preset through hole 2 on the silk fibroin membrane 1; filling the preset through hole 2 with conductive ink; the conductive ink is an aqueous solution of a polymer formed by silk fibroin and carbon nanotubes; and then performing a first drying treatment to form the conductive hole 3.
[0078] In the embodiment of the present application, the method for preparing the conductive ink may specifically include:
[0079] The silk fibroin aqueous solution and the carbon nanotube aqueous solution are mixed according to a preset ratio; the preset ratio satisfies that the mass ratio of the silk fibroin to the carbon nanotube is 0.5 to 0.9; the mixed solution of the silk fibroin aqueous solution and the carbon nanotube aqueous solution is heated to a preset temperature, and stirred at a low speed to obtain a conductive ink.
[0080] The silk fibroin aqueous solution can be prepared based on the above steps 1)-5), and optionally, the mass fraction of the silk fibroin aqueous solution is 1.5% to 3.5%. Exemplarily, the mass fraction of the silk fibroin aqueous solution can be 1.5%, 2%, 2.5%, 3% or 3.5%.
[0081] The carbon nanotube aqueous solution can be specifically achieved through the following steps: providing a predetermined amount of carbon nanotubes; adding the carbon nanotubes into deionized water to obtain a carbon nanotube mixed solution; subjecting the carbon nanotube mixed solution to ultrasonic treatment, stirring treatment and centrifugal treatment in sequence to obtain an initial carbon nanotube aqueous solution; and diluting the initial carbon nanotube aqueous solution to obtain a carbon nanotube aqueous solution.
[0082] In the embodiment of the present application, a predetermined amount of carbon nanotubes is slowly added to deionized water to obtain a carbon nanotube mixed solution. The carbon nanotube mixed solution is subjected to ultrasonic treatment, stirring treatment and centrifugal treatment in sequence to obtain an initial carbon nanotube aqueous solution in which the carbon nanotubes are uniformly dispersed. In order to obtain the initial carbon nanotube aqueous solution, the carbon nanotube mixed solution is first subjected to ultrasonic treatment using an ultrasonic processor to break up the aggregates of the carbon nanotubes and improve the dispersibility of the carbon nanotubes; the carbon nanotube mixed solution is then stirred using a magnetic stirrer to enhance the dispersion effect of the carbon nanotubes; and the carbon nanotube mixed solution is then subjected to high-speed centrifugal treatment to remove undispersed large particles or aggregates in the carbon nanotube mixed solution. The supernatant of the solution after centrifugation is the initial carbon nanotube aqueous solution.
[0083] Optionally, the ultrasonic treatment time is 15 to 45 minutes. Exemplarily, the ultrasonic treatment time can be 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes or 45 minutes.
[0084] Optionally, the stirring treatment time is 10 to 14 hours. Exemplarily, the stirring treatment time can be 10 hours, 11 hours, 12 hours, 13 hours or 14 hours.
[0085] Optionally, the centrifugal treatment time is 15 to 30 minutes. Exemplarily, the centrifugal treatment time can be 15 minutes, 20 minutes, 25 minutes or 30 minutes.
[0086] In the examples of the present application, the ultrasonic treatment time is 15 min, the stirring treatment time is 12 h, and the centrifugal treatment time is 22 min.
[0087] In the embodiment of the present application, the initial carbon nanotube aqueous solution is diluted to obtain a carbon nanotube aqueous solution. The mass fraction of the carbon nanotube aqueous solution needs to be controlled within a certain range so that the carbon nanotube aqueous solution can be fully mixed with the silk fibroin aqueous solution and the conductivity of the carbon nanotubes can be fully exerted. If the mass fraction of the carbon nanotube aqueous solution is too high, there will not be enough solvent to promote the recombination of carbon nanotubes in the silk fibroin molecular network. If the mass fraction of the carbon nanotube aqueous solution is too low, the carbon nanotube content in the mixed solution formed by mixing the silk fibroin aqueous solution and the carbon nanotube aqueous solution is too low, resulting in poor conductivity of the mixed solution.
[0088] In the embodiments of the present application, the mass fraction of the carbon nanotube aqueous solution needs to be precisely controlled, and the mass fraction of the initial carbon nanotube aqueous solution used to configure the carbon nanotube aqueous solution and the mass fraction of the carbon nanotube mixed solution used to configure the initial carbon nanotube aqueous solution can be controlled within a certain range. However, it is necessary to ensure that the mass fraction of the initial carbon nanotube aqueous solution and the mass fraction of the carbon nanotube mixed solution are greater than the mass fraction of the carbon nanotube aqueous solution, so as not to affect the configuration of the carbon nanotube aqueous solution. Since the centrifugal treatment step will discard some carbon nanotubes in the process of configuring the initial carbon nanotube aqueous solution using the carbon nanotube mixed solution, the mass fraction of the initial carbon nanotube aqueous solution cannot be equated with the mass fraction of the carbon nanotube mixed solution. In this regard, a moisture balance can be used to determine the mass fraction of the initial carbon nanotube aqueous solution, and a carbon nanotube aqueous solution of the required mass fraction can be configured.
[0089] Optionally, the mass fraction of the carbon nanotube mixture is 2.5% to 7.5%. Exemplarily, the mass fraction of the carbon nanotube mixture can be 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7% or 7.5%.
[0090] Optionally, the mass fraction of the carbon nanotube aqueous solution is 1% to 3%. Exemplarily, the mass fraction of the carbon nanotube aqueous solution can be 1%, 1.5%, 2%, 2.5% or 3%.
[0091] Optionally, the mass fraction of the carbon nanotube aqueous solution is 1%. Optionally, the mass fraction of the carbon nanotube aqueous solution is 2%. Optionally, the mass fraction of the carbon nanotube aqueous solution is 3%.
[0092] In the embodiment of the present application, the carbon nanotubes are multi-walled carbon nanotubes. Multi-walled carbon nanotubes are easy to prepare, low in cost, suitable for mass production, and multi-walled carbon nanotubes have a relatively large diameter, making it easier to form a stable conductive network during the dispersion process.
[0093] In a feasible embodiment, the carbon nanotubes may also be single-walled carbon nanotubes. Single-walled carbon nanotubes can provide higher conductivity, but their preparation cost is higher and their dispersion is more difficult to prepare.
[0094] In a feasible implementation, taking into account the conductive properties and the preparation cost, the carbon nanotubes may be a mixture of single-walled carbon nanotubes and multi-walled carbon nanotubes.
[0095] In the embodiment of the present application, the silk fibroin aqueous solution and the carbon nanotube aqueous solution are first mixed according to a preset ratio, and then the mixed solution of the silk fibroin aqueous solution and the carbon nanotube aqueous solution is heated to a preset temperature, and subjected to a low-speed stirring treatment to obtain a conductive ink. This process adopts a low-speed stirring treatment so that the silk fibroin aqueous solution and the carbon nanotube aqueous solution are fully mixed. This process needs to avoid vigorous stirring to prevent the silk fibroin from cross-linking to form a gel.
[0096] In the embodiment of the present application, when the silk fibroin aqueous solution and the carbon nanotube aqueous solution are just mixed together, the carbon nanotubes are not well dispersed in the silk fibroin solution, and the mixed solution will show obvious stratification. After low-speed stirring, the carbon nanotubes will gradually disperse in the silk fibroin solution and eventually form a uniform conductive ink. In the conductive ink, the amino acid residues (such as hydroxyl, carboxyl, amino, etc.) in the silk fibroin can form hydrogen bonds with the functional groups (such as carboxyl, hydroxyl) present on the surface of the carbon nanotubes. Moreover, the functional groups of the silk fibroin may undergo cross-linking reactions with the functional groups in the carbon nanotubes.
[0097] In the embodiment of the present application, the silk fibroin aqueous solution and the carbon nanotube aqueous solution are mixed according to a preset ratio, and the mass ratio of the silk fibroin and the carbon nanotube in the conductive ink is required to be within a certain range. The difference in the mass ratio of silk fibroin and the carbon nanotube will result in different conductive properties and biocompatibility of the conductive ink. If the mass ratio of silk fibroin and the carbon nanotube is lower than the preset ratio, the content of silk fibroin is too low, and the content of carbon nanotube is too high, the biocompatibility of the conductive ink will be poor. If the mass ratio of silk fibroin and the carbon nanotube is higher than the preset ratio, the content of silk fibroin is too high, and the content of carbon nanotube is too low, the silk fibroin aqueous solution will be difficult to fully mix with the carbon nanotube aqueous solution, and it is easy to cause the two to mix to form a gel-like substance, resulting in the conductive ink formed by the silk fibroin aqueous solution and the carbon nanotube aqueous solution having poor conductivity.
[0098] In a feasible embodiment, the preset ratio satisfies that the mass ratio of silk fibroin to carbon nanotubes is 0.5 to 0.9, that is, the mass ratio of silk fibroin to carbon nanotubes in the silk fibroin aqueous solution and the carbon nanotube aqueous solution used to prepare the conductive ink is 0.5 to 0.9. Exemplarily, the mass ratio of silk fibroin to carbon nanotubes can be 0.5, 0.6, 0.7, 0.8 or 0.9.
[0099] In a feasible embodiment, the preset temperature is 32-42° C. Exemplarily, the preset temperature may be 32° C., 33° C., 34° C., 35° C., 36° C., 37° C., 38° C., 39° C., 40° C., 41° C. or 42° C.
[0100] In a feasible embodiment, the low-speed stirring treatment time is 10 to 20 minutes. Exemplarily, the low-speed stirring treatment time can be 10 minutes, 15 minutes or 20 minutes.
[0101] In a feasible embodiment, the pH value of the solution after the silk fibroin aqueous solution and the carbon nanotube aqueous solution are mixed can also be adjusted to meet different application requirements. The charge state of silk fibroin depends on the pH value of the solution. Near the isoelectric point (pH about 4.5), the net charge of silk fibroin is zero and the solubility is the lowest. Under acidic conditions, silk fibroin is positively charged; under alkaline conditions, silk fibroin is negatively charged. These charge changes will affect the electrostatic interaction between silk fibroin and carbon nanotubes, thereby affecting the stability and conductivity of the mixed solution.
[0102] In the embodiment of the present application, a silk fibroin aqueous solution with a mass fraction of 2.5% and a carbon nanotube aqueous solution with a mass fraction of 2% are selected. According to the standard that the mass ratio of silk fibroin to carbon nanotube is 0.7, appropriate amounts of silk fibroin aqueous solution and carbon nanotube aqueous solution are mixed, the mixed solution is heated to 37°C, and stirred at a low speed for 20 minutes to obtain a conductive ink. Among them, the pH value of the mixed solution is not adjusted, and the mixed solution of the silk fibroin aqueous solution and the carbon nanotube aqueous solution is a neutral solution.
[0103] In a feasible embodiment, the predetermined through hole 2 is formed on the silk fibroin film 1, comprising: providing two blocking members; placing a blocking member on the upper and lower surfaces of the silk fibroin film 1 respectively to form an intermediate structure; the size of the blocking member is greater than or equal to the size of the silk fibroin film 1; and using a laser punching process to form a predetermined through hole 2 on the intermediate structure, so as to obtain the following. Figure 2 The structure shown.
[0104] In the embodiment of the present application, the material of the blocking member includes polyvinyl alcohol, which can also be a material with similar properties to the silk fibroin membrane 1, that is, it can become soft when exposed to water and has a certain degree of stretchability, but does not adhere to the silk fibroin membrane 1, so that the blocking member can be removed from the target silk fibroin membrane 1 after the hole filling is completed.
[0105] In a feasible embodiment, the conditions of the first drying treatment include: a drying temperature of 40 to 50° C. and a drying time of 1 to 3 hours. Room temperature drying may also be used, but the drying time is longer, requiring at least 1 day.
[0106] In a feasible embodiment, the diameter of the preset through hole 2 is 0.05-0.2 mm.
[0107] In an embodiment of the present application, the process parameters of the laser punching process may include: a punching speed of 600 to 750 mm / s; a frequency of 45 to 55 kHz; a pulse width of 0.5 to 1.5 μs; and a laser scanning density of 0.015 to 0.03 mm.
[0108] In the embodiment of the present application, there are two schemes for preparing the metal pattern layer 4 on the silk fibroin film 1. One is to use an electron beam evaporation process, specifically, by forming a mask pattern on the silk fibroin film 1; using electron beam evaporation technology to evaporate the metal pattern layer 4 onto the silk fibroin film 1 through the mask pattern, and removing the mask pattern. The other is a screen printing process, specifically, using screen printing technology to scrape the conductive ink onto the silk fibroin film 1; and then performing a second drying process to form the metal pattern layer 4. Optionally, the conditions of the second drying process include: a drying temperature of 40 to 50°C and a drying time of 1 to 3 hours.
[0109] In the embodiment of the present application, the conductive material filling the preset through hole 2 is conductive ink. Since the conductive ink is prepared from a silk fibroin aqueous solution and carbon nanotubes, the amino acid residues (such as hydroxyl, carboxyl, amino, etc.) in the silk fibroin in the silk fibroin film can form hydrogen bonds with the functional groups (such as carboxyl, hydroxyl) on the surface of the carbon nanotubes, and the black conductive layer formed by the conductive ink and the base layer formed by the silk fibroin film have good adhesion reliability and will not fall off. Similarly, when the metal pattern layer 4 is formed by conductive ink, it also has the above-mentioned effect, so that the entire multi-layer conductive structure can not only realize the design of complex circuits, but also has better biocompatibility, mechanical properties and degradability.
[0110] S105: bonding the at least two target silk fibroin films according to a preset structural hierarchy to form a multilayer conductive structure;
[0111] In a feasible embodiment, step S103 may specifically include: performing plasma cleaning treatment on at least two of the target silk fibroin films 1 respectively; coating silk fibroin liquid on the surfaces to be bonded in at least two of the target silk fibroin films 1 respectively; stacking and pressing at least two of the target silk fibroin films 1 according to a preset structural hierarchy to obtain an initial multi-layer conductive structure; and sequentially performing water vapor crosslinking and drying treatment on the initial multi-layer conductive structure to obtain the multi-layer conductive structure.
[0112] Optionally, the parameters of the plasma cleaning treatment are: power of 35 to 45 W; time of 25 to 35 s. Optionally, for N target silk fibroin films 1, the silk fibroin solution can be applied only on the upper / lower surface of N-1 protein films, where N is an integer greater than or equal to 2. Continuing with the above example, for example Figure 3 The two target silk fibroin membranes 1 shown can be prepared by coating the upper surface of the first silk fibroin membrane 11 with silk fibroin liquid, and then covering the lower surface of the second silk fibroin membrane 12 on the upper surface of the first silk fibroin membrane 11. The two target silk fibroin membranes 1 can be pressed tightly using a silicone pad, and then placed in a vacuum kettle containing water for steam cross-linking treatment. The specific parameters of the steam cross-linking treatment can be found in the description of the above-mentioned preparation of the silk fibroin membrane 1.
[0113] An embodiment of the present application provides a method for preparing a multi-layer conductive structure, wherein a plurality of target silk fibroin films 1 are obtained by punching and filling each silk fibroin film 1 with conductive ink to form conductive holes 3 and a metal pattern layer 4, and then the plurality of target silk fibroin films 1 are bonded together according to a preset stacking order and a reference for aligning the conductive holes 3 of the upper and lower target silk fibroin films 1, thereby obtaining a multi-layer conductive structure.
[0114] Silk fibroin is a natural protein with good biocompatibility and biodegradability. In the fields of medicine and bioelectronics, silk fibroin is used as a substrate material to prepare conductive structures compatible with human tissue for use in biosensors, implantable medical devices, etc.
[0115] Silk fibroin has excellent mechanical strength and elasticity. This allows silk fibroin-based multilayer conductive structures to not only withstand a certain amount of physical pressure, but also maintain functionality when bent and stretched, making them suitable for wearable devices and flexible electronic products.
[0116] This solution not only has a simple preparation process, but also has the advantages of good biocompatibility, good mechanical properties and degradability because the multilayer conductive structure prepared by the present application is based on the above-mentioned silk fibroin film 1, and the conductive ink filled in the conductive hole 3 is an aqueous solution of a polymer formed by silk fibroin and carbon nanotubes, so that the overall conductive performance is highly reliable, showing great application prospects in the fields of biomedicine, environmental protection and wearable devices. The development of this technology helps to promote the development of traditional electronic manufacturing in a greener and more sustainable direction.
[0117] On the other hand, the present application further discloses a conductive structure, which is prepared using the above-mentioned preparation method.
[0118] The present application further discloses an electronic device, which includes the above conductive structure. Specifically, the electronic device can be an electronic device applied in the field of biomedicine and wearable devices, such as a biosensor, an implantable device, etc.
[0119] The above description is only an optional embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a multilayer conductive structure, characterized in that: include: providing at least two silk fibroin films; Preparing conductive holes and a metal pattern layer on each of the at least two silk fibroin films to obtain at least two target silk fibroin films; Bonding the at least two target silk fibroin films according to a preset structural hierarchy to form a multi-layer conductive structure; Wherein, preparing conductive holes on each of the silk fibroin membranes comprises: forming a preset through hole on the silk fibroin film; Filling the preset through hole with conductive ink; the conductive ink is an aqueous solution of a polymer formed by silk fibroin and carbon nanotubes; Then, a first drying process is performed to form the conductive hole.
2. The preparation method according to claim 1, characterized in that: The method of forming a preset through hole on the silk fibroin film comprises: Two blocking members are provided; Placing a blocking member on the upper and lower surfaces of the silk fibroin film respectively to form an intermediate structure; the size of the blocking member is greater than or equal to the size of the silk fibroin film; A laser punching process is used to form a preset through hole on the intermediate structure.
3. The preparation method according to claim 1, characterized in that: The conditions of the first drying process include: The drying temperature is 40-50°C and the drying time is 1-3 hours.
4. The preparation method according to claim 2, characterized in that: The diameter of the preset through hole is 0.05-0.2 mm; The material of the barrier member includes polyvinyl alcohol.
5. The preparation method according to claim 1, characterized in that: Preparing a metal graphic layer on each of the silk fibroin films, comprising: forming a mask pattern on the silk fibroin film; The metal pattern layer is formed by evaporating the metal onto the silk fibroin film through the mask pattern using electron beam evaporation technology, and the mask pattern is removed.
6. The preparation method according to claim 1, characterized in that: Preparing a metal graphic layer on each of the silk fibroin films, comprising: Using screen printing technology to scrape the conductive ink onto the silk fibroin film; A second drying process is then performed to form the metal pattern layer.
7. The preparation method according to claim 1, characterized in that: The step of bonding the at least two target silk fibroin films according to a preset structural hierarchy to form a multi-layer conductive structure comprises: performing plasma cleaning treatment on at least two of the target silk fibroin films respectively; Coating the silk fibroin solution on the surfaces to be bonded in at least two of the target silk fibroin films respectively; stacking and pressing at least two of the target silk fibroin films according to a preset structural hierarchy to obtain an initial multi-layer conductive structure; The initial multi-layer conductive structure is subjected to steam cross-linking and drying treatments in sequence to obtain the multi-layer conductive structure.
8. The preparation method according to claim 1, characterized in that: The step of preparing conductive holes and a metal pattern layer on each of the at least two silk fibroin films to obtain at least two target silk fibroin films comprises: Conductive holes are prepared on each of the at least two silk fibroin membranes, and a metal pattern layer is prepared on each of the silk fibroin membranes to obtain at least two target silk fibroin membranes; or a metal pattern layer is prepared on each of the at least two silk fibroin membranes, and a conductive hole is prepared on each of the silk fibroin membranes to obtain at least two target silk fibroin membranes.
9. A conductive structure, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 8.
10. An electronic device, characterized in that: Comprising the conductive structure as claimed in claim 9.
Citation Information
Patent Citations
Silk fibroin / graphene composite conductive film and preparation method thereof
CN109880382A
Silver nanothread / silk fibroin composite fiber and preparation method thereof
CN110230113A
Transparent conductive film and preparation method thereof
CN110364303A
Protein conductive ink, protein device and preparation method
CN117210064A