Method for cleaning silicon carbide substrate polishing solution by using common strong oxidant
By using reducing agents and precipitants in acidic and alkaline environments, combined with ultrasonic and mechanical brushing, hydrofluoric acid etching and nitrogen blow-drying, the problem of incomplete cleaning of permanganate decomposition products in the prior art is solved, and the problem of incomplete cleaning of permanganate decomposition products is achieved. Efficient cleaning of silicon carbide substrate polishing liquid.
Patent Information
- Application Number
- CN202411019966.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art cannot effectively clean the permanganate and its decomposition products, resulting in incomplete cleaning of the silicon carbide substrate polishing liquid.
Use acidic environment and reducing agent to remove MnO42-ions, alkaline environment and precipitant to remove Mn2+ and Na+/K+ ions, and use hydrofluoric acid to etch the oxide layer, combined with mechanical brushing and nitrogen blow-drying, to achieve thoroughness of the wafer surface Clean.
Effectively remove residual particles and ions on the wafer surface after polishing, ensuring thorough cleaning without introducing new impurity ions, and improving the cleaning effect of silicon carbide substrate polishing liquid.
Smart Images

Figure CN119008379A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wafer strong oxidant cleaning, and more specifically, relates to a cleaning method using a strong oxidant commonly used in a silicon carbide substrate polishing liquid. Background Art
[0002] The Mohs hardness of silicon carbide substrate material is relatively high, and it is very difficult to directly remove the silicon carbide substrate material. Therefore, the method of oxidation first and then removal is often used in the polishing process. Commonly used oxidants in silicon carbide polishing liquid include strong oxidants such as potassium permanganate, sodium permanganate and hydrogen peroxide. However, permanganate is often used as an oxidant for silicon carbide polishing due to its super strong oxidizing property. During the polishing process, permanganate will decompose in the polishing liquid, but during the wafer cleaning process, permanganate is usually cleaned, and the products after the decomposition of permanganate cannot be effectively cleaned, resulting in incomplete cleaning. Summary of the invention
[0003] The object of the present invention is to provide a cleaning method of a silicon carbide substrate polishing liquid using a common strong oxidant, aiming to solve the problem that the existing cleaning method cannot effectively clean permanganate and its decomposition products.
[0004] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for cleaning a silicon carbide substrate polishing liquid with a commonly used strong oxidant, comprising the following steps:
[0005] Remove particles and residual MnO4 from the wafer surface 2- ion;
[0006] Remove residual Mn on the wafer surface 2+ and Na + / K + ion;
[0007] Etching the oxide layer on the surface of the wafer; and
[0008] Dry the wafer surface.
[0009] In one possible implementation, the particles and residual MnO4 on the wafer surface are removed. 2- ions, including:
[0010] Place the wafer in an acidic environment and add a reducing agent to precipitate the MnO4 remaining on the wafer surface. 2- ions; and
[0011] At the same time, the wafer is cleaned with ultrasonic waves to remove particles from the surface of the wafer.
[0012] In a possible implementation, the pH value of the acidic environment is 2-4, and the concentration of the reducing agent is 0.3 wt %-3 wt %.
[0013] In a possible implementation, the power of the ultrasonic wave is 200W-500W.
[0014] In one possible implementation, the residual Mn on the wafer surface is removed. 2+ and Na + / K + ions, including:
[0015] Place the wafer in an alkaline environment to remove Mn 2+ ion;
[0016] Add precipitant to remove Na + / K + ions; and
[0017] The wafer is placed in an alkaline environment and mechanically scrubbed at the same time.
[0018] In a possible implementation, the pH value of the alkaline environment is 8-10, and the concentration of the precipitant is 0.5 wt%-2 wt%.
[0019] In a possible implementation, etching an oxide layer on a surface of a wafer includes:
[0020] The wafer is placed in hydrofluoric acid for etching and mechanical scrubbing at the same time, wherein the concentration of the hydrofluoric acid is 3000ppm-6000ppm.
[0021] In a possible implementation, drying the wafer surface includes:
[0022] Rotate the wafer to remove liquid from the wafer surface using centrifugal force; and
[0023] A nitrogen gas flow is used to purge the wafer surface.
[0024] In a possible implementation, when the wafer is rotated, the rotation speed of the wafer is 300 r / min-1200 r / min.
[0025] In a possible implementation, the flow rate of the nitrogen gas flow is 20 L / min-60 L / min, and the angle between the nitrogen gas flow and the wafer is 5°-10°.
[0026] The cleaning method of the silicon carbide substrate polishing liquid commonly used with a strong oxidant provided by the present invention has the beneficial effect that: compared with the prior art, the cleaning method of the silicon carbide substrate polishing liquid commonly used with a strong oxidant of the present invention can remove the residual particles on the surface of the wafer while gradually and directionally cleaning the MnO4 generated by the decomposition of permanganate. 2 , Mn 2+ and Na + / K+ ions without introducing new impurity ions, and can effectively clean the polished wafer. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 A schematic diagram of the main steps of a cleaning method using a strong oxidant commonly used in a silicon carbide substrate polishing liquid provided by an embodiment of the present invention;
[0029] Figure 2 The present invention provides a method for removing particles and residual MnO4 on the surface of a wafer. 2- Schematic diagram of the main steps of ion;
[0030] Figure 3 The present invention provides a method for removing residual Mn from the surface of a wafer. 2+ and Na + / K + Schematic diagram of the main steps of ion;
[0031] Figure 4 A schematic diagram of the main steps of drying the wafer surface provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0032] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0033] Reference Figure 1 and Figure 4 The cleaning method of the silicon carbide substrate polishing liquid using a commonly used strong oxidant provided by the present invention is now described. The cleaning method of the silicon carbide substrate polishing liquid using a commonly used strong oxidant comprises the following steps:
[0034] S1. Remove particles and residual MnO4 on the wafer surface 2- ion.
[0035] S2. Remove the residual Mn on the wafer surface 2+ and Na + / K + ion.
[0036] S3. Etching the oxide layer on the surface of the wafer.
[0037] S4. Dry the wafer surface.
[0038] The cleaning method of the silicon carbide substrate polishing liquid provided by the present invention with a common strong oxidant can remove the residual particles on the surface of the wafer and gradually and directionally clean the MnO4 generated by the decomposition of permanganate. 2 , Mn 2+ and Na + / K + ions without introducing new impurity ions, and can effectively clean the polished wafer.
[0039] Optionally, step S1. specifically includes the following steps:
[0040] S11. Place the wafer in an acidic environment and add a reducing agent to precipitate the MnO4 remaining on the wafer surface. 2- ion.
[0041] S12. At the same time, the wafer is cleaned by ultrasonic wave so that particles on the surface of the wafer fall off.
[0042] Optionally, the pH value of the acidic environment in step S11 is 2-4, and the concentration of the reducing agent is 0.3wt-3wt%. The acidic environment is mainly provided by an acidic pH reagent, and the acidic pH reagent includes but is not limited to sulfuric acid, citric acid, formic acid, and nitric acid. 2- The ions will be reduced to Mn by the reducing agent in an acidic environment. 2+ Ions. The reducing agent is mainly a less oxidizing agent than MnO4 2- Reagents of substances, reducing agents include but are not limited to ferrous salts, ammonia, hydrogen peroxide, and hydrides.
[0043] Optionally, in step S12, when ultrasonic cleaning is used, the power of the ultrasonic wave is 200 W-500 W. The wafer is immersed in an acidic reagent, and the ultrasonic wave generates a large number of bubbles in the acidic reagent. The shock wave generated when the bubbles break causes the wafer to resonate, thereby causing particles attached to the surface of the wafer to fall off.
[0044] Optionally, step S2 specifically includes the following steps:
[0045] S21. Place the wafer in an alkaline environment to remove Mn 2+ ion.
[0046] S22. Add precipitant to remove Na + / K + ion.
[0047] S23. Place the wafer in an alkaline environment and perform mechanical scrubbing at the same time.
[0048] Optionally, the pH value of the alkaline environment in step S21. is 8-10, and the concentration of the precipitant in step S22. is 0.5wt%-2wt%. Mn 2+ In an alkaline environment, it will hydroxylate to form trivalent manganese ion Mn(OH)3 precipitation, Na + / K + Under the action of precipitant (alkaline environment), ions generate sodium salt precipitate, thereby removing the ions.
[0049] Optionally, etching the oxide layer on the surface of the wafer in step S3. specifically includes:
[0050] The wafer is placed in hydrofluoric acid for etching and mechanical scrubbing at the same time. The concentration of hydrofluoric acid is 3000ppm-6000ppm. The hydrofluoric acid etches away a thin layer of oxide layer on the surface of the wafer, thus exposing the surface of the wafer.
[0051] Optionally, step S4 specifically includes the following steps:
[0052] S41. Rotate the wafer and use centrifugal force to remove the liquid on the surface of the wafer.
[0053] S42. Purge the wafer surface using a nitrogen gas flow.
[0054] Optionally, when the wafer is rotated in step S41, the rotation speed of the wafer is 300r / min-1200r / min.
[0055] Optionally, in step S42, the flow rate of the nitrogen gas flow is 20 L / min-60 L / min, and the angle between the nitrogen gas flow and the wafer is 5°-10°. The nitrogen gas outlet moves from the center of the wafer to the edge, so that the wafer is dried.
[0056] In a preferred embodiment, this embodiment provides a method for cleaning a silicon carbide substrate polishing liquid using a common strong oxidant.
[0057] Currently, integrated circuits (ICs) all use silicon-based substrate materials. However, with the increasing demand for RF devices and high-frequency devices, the third-generation semiconductor material silicon carbide has become the first choice for RF devices and power devices. Silicon carbide materials have the advantages of stable chemical properties, high thermal conductivity, small thermal expansion coefficient and good wear resistance. Therefore, silicon carbide is often used in new energy vehicles, 5G communications and other advanced technologies. As an important component of silicon carbide devices, the processing of silicon carbide substrates includes raw material synthesis, crystal growth, ingot processing, crystal rod cutting, wafer thinning, polishing and cleaning.
[0058] The Mohs hardness (9.5) of silicon carbide substrate material is relatively high, and it is very difficult to directly remove the silicon carbide substrate material. Therefore, the method of first oxidation and then removal is often used in the polishing process. Commonly used oxidants in silicon carbide polishing liquid include strong oxidants such as potassium permanganate, sodium permanganate and hydrogen peroxide. However, permanganate (potassium permanganate, sodium permanganate, etc.) is often used as an oxidant for silicon carbide polishing due to its super strong oxidizing property. Among them, the pollution of the cleaning process mainly comes from the polishing liquid used for silicon carbide substrate polishing. Therefore, this embodiment provides a cleaning method of silicon carbide substrate material using a commonly used strong oxidant.
[0059] Sodium permanganate / potassium permanganate mainly produces Na by decomposition and redox reaction in acidic polishing liquid (pH between 2-4). + , K + 、MnO4 2- , MnO2 and other substances, so these substances need to be cleaned and removed. The post-CMP cleaning technology mainly includes four steps: Mega (ultrasonic cleaning), Brush 1 (mechanical brushing), Brush 2 (mechanical brushing) and Dryer (drying chamber). This patent will analyze the four cleaning steps.
[0060] First, the Mega chamber uses 200W-500W ultrasonic vibration to remove the MnO2 and other particles on the wafer. The shock wave generated by the bubbles in the Mega chamber resonates with the wafer, causing the remaining particles on the wafer to fall off. At the same time, an acidic cleaning solution plus a reducing agent is used to remove the remaining MnO4 2- In acidic environment, MnO4 2- The substance will be reduced to Mn 2+ ions, which can effectively reduce MnO4 2- The acidic environment with a pH value of 2-4 is mainly provided by an acidic pH reagent, which includes but is not limited to sulfuric acid, citric acid, formic acid and nitric acid. The concentration of the reducing agent is 0.3wt%-3wt%, and the reducing agent is mainly an oxidizing agent with a lower oxidizing property than MnO4 2- Reagents of substances, reducing agents include but are not limited to ferrous salts, ammonia, hydrogen peroxide and hydrides, etc.
[0061] Secondly, the Brush 1 (mechanical brushing) chamber uses an alkaline environment with a pH value of 8-10 and Na + / K + The concentration of the precipitant is 0.5wt%-2wt%. The purpose of this step is to remove Mn 2+ and Na + / K + ions. In alkaline environment, Mn 2+The ions will undergo hydrolysis to generate hydroxylated trivalent manganese ions Mn(OH)3 precipitate. + / K + The ions generate sodium salt precipitates under the action of precipitants and alkaline environment.
[0062] Secondly, the Brush 2 (mechanical brushing) chamber uses etching agents such as hydrofluoric acid with a concentration of 3000ppm-6000ppm to etch away a thin layer of oxide layer on the surface of silicon carbide, thereby exposing the surface of silicon carbide.
[0063] Finally, the wafer surface is dried by the Dryer (drying chamber). The wafer is dried by high-speed rotation. The rotation speed of the wafer is 300r / min-1200r / min. At the same time, the wafer surface is purged with high-purity nitrogen to achieve the purpose of drying. The nitrogen flow rate is 20L / min-60L / min, and the nitrogen outlet is tilted at an angle of 5°-20°. The nitrogen outlet moves from the center of the wafer to the edge, so that the wafer is dry.
[0064] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A cleaning method for a silicon carbide substrate polishing liquid using a common strong oxidant, characterized in that: The following steps are involved: Remove particles and residual MnO4 from the wafer surface 2- ion; Remove residual Mn on the wafer surface 2+ and Na + / K + ion; Etching the oxide layer on the surface of the wafer; And drying the wafer surface.
2. The cleaning method of silicon carbide substrate polishing liquid commonly used strong oxidant according to claim 1, characterized in that: Remove particles and residual MnO4 from the wafer surface 2- ions, including: Place the wafer in an acidic environment and add a reducing agent to precipitate the MnO4 remaining on the wafer surface. 2- ions; and At the same time, the wafer is cleaned with ultrasonic waves to remove particles from the surface of the wafer.
3. The cleaning method of silicon carbide substrate polishing liquid commonly used strong oxidant as claimed in claim 2, characterized in that: The pH value of the acidic environment is 2-4, and the concentration of the reducing agent is 0.3wt-3wt%.
4. The cleaning method of silicon carbide substrate polishing liquid commonly used strong oxidant as claimed in claim 2, characterized in that: The power of the ultrasonic wave is 200W-500W.
5. The cleaning method of silicon carbide substrate polishing liquid commonly used strong oxidant as claimed in claim 1, characterized in that: Remove residual Mn on the wafer surface 2+ and Na + / K + ions, including: Place the wafer in an alkaline environment to remove Mn 2+ ion; Add precipitant to remove Na + / K + ions; and The wafer is placed in an alkaline environment and mechanically scrubbed at the same time.
6. The cleaning method of silicon carbide substrate polishing liquid commonly used strong oxidant as claimed in claim 5, characterized in that: The pH value of the alkaline environment is 8-10, and the concentration of the precipitant is 0.5wt%-2wt%.
7. The cleaning method of silicon carbide substrate polishing liquid commonly used strong oxidant as claimed in claim 1, characterized in that: Etching the oxide layer on the wafer surface, including: The wafer is placed in hydrofluoric acid for etching and mechanical scrubbing at the same time, wherein the concentration of the hydrofluoric acid is 3000ppm-6000ppm.
8. The cleaning method of silicon carbide substrate polishing liquid commonly used strong oxidant as claimed in claim 1, characterized in that: Dry the wafer surface, including: Rotate the wafer to remove liquid from the wafer surface using centrifugal force; and A nitrogen gas flow is used to purge the wafer surface.
9. The cleaning method of silicon carbide substrate polishing liquid commonly used strong oxidant as claimed in claim 8, characterized in that: When the wafer is rotated, the rotation speed of the wafer is 300r / min-1200r / min.
10. The cleaning method of silicon carbide substrate polishing liquid commonly used strong oxidant according to claim 8, characterized in that: The flow rate of the nitrogen gas flow is 20L / min-60L / min, and the angle between the nitrogen gas flow and the wafer is 5°-10°.