Semiconductor ohmic contact processing system and method based on laser annealing
By using laser annealing technology combining large-size flat-top light and one-direction blowing in the ohmic contact manufacturing of silicon carbide, the low efficiency and unevenness problems in traditional methods are solved, and efficient and uniform ohmic contact structure processing is achieved.
Patent Information
- Application Number
- CN202411082380.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
In traditional silicon carbide ohmic contact manufacturing, rapid thermal annealing is difficult to accurately control the annealing area and depth. Laser annealing is inefficient and costly during large-area processing, and there is local unevenness in scanning areas.
Large-size flat top light is used as the laser annealing light source, combined with single-direction blowing and defocus scanning technology, to reduce the number of spot movements, improve processing efficiency, and uniformize the beam distribution through defocusing to solve the problem of uneven scanning areas.
It greatly improves processing efficiency, ensures uniformity of large-area surface morphology, reduces costs, and improves the quality and reliability of ohmic contacts.
Smart Images

Figure CN119008392A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of silicon carbide manufacturing, and in particular relates to a semiconductor ohmic contact processing system and method based on laser annealing. Background Art
[0002] Silicon carbide (SiC), as a wide bandgap semiconductor material, is widely used in high-power and high-frequency electronic devices due to its excellent thermal conductivity, high breakdown electric field strength, and high electron saturation drift velocity. These unique properties make silicon carbide an ideal candidate material for high-power and high-temperature electronic devices, especially in application scenarios where traditional semiconductor materials such as silicon cannot meet the requirements.
[0003] The formation of low-resistance and thermally stable ohmic contacts on silicon carbide is critical to the performance and life of silicon carbide-based devices. Ohmic contacts ensure that charge carriers are efficiently injected from metals into semiconductors without introducing significant energy barriers or excessive resistance. This efficient charge transfer is essential to maintaining the overall functionality and efficiency of electronic devices; poor ohmic contacts can lead to excessive contact resistance, increased power loss, and reduced device reliability, ultimately affecting the performance of the entire electronic system.
[0004] At present, the main technologies for manufacturing silicon carbide ohmic contacts are rapid thermal annealing and laser thermal annealing. However, it is difficult to accurately control the annealing area and depth as well as the microstructural characteristics of the contact area with traditional rapid thermal annealing. To overcome these challenges, laser annealing is a promising method, which has the advantages of local heating, minimal substrate damage, and precise control of annealing parameters. Moreover, laser annealing will not affect the device structure on the front side of the wafer. Therefore, the front device structure can be manufactured first, then the wafer is thinned, and finally the required ohmic contact is formed by laser annealing on the back side. Wafer thinning is crucial to reducing the power loss of power devices.
[0005] When using laser annealing to manufacture silicon carbide ohmic contacts, in addition to ensuring the quality of the ohmic contacts, process efficiency is also a key factor in the successful transfer of this technology to actual industrial applications. Currently, laser annealing technology mostly uses small-sized spots. Although small spots can achieve more precise control, when processing large areas, more scans and longer processing times are required, which will lead to higher costs and lower efficiency in commercial production. Summary of the invention
[0006] The purpose of the present invention is to provide a semiconductor ohmic contact processing method based on laser annealing, which can at least solve some of the defects existing in the prior art.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] A semiconductor ohmic contact processing method based on laser annealing. When laser annealing is performed on the surface of a semiconductor sample, a large-size flat-top light is used as an annealing light source to emit to the surface of the semiconductor sample, and air is blown in a single direction on the surface of the semiconductor sample, and the blowing direction is the same as the stepping direction of the semiconductor sample.
[0009] Furthermore, when the large-size flat-top light is emitted to the surface of the semiconductor sample, the surface of the silicon carbide sample is scanned in a defocused manner.
[0010] Furthermore, the defocus amount of the defocus scanning is 50-1000 μm.
[0011] Furthermore, the laser M of the laser annealing treatment 2 The factor is greater than 10.
[0012] Furthermore, the laser center wavelength of the laser annealing treatment is 200-400 nm, the repetition frequency is 1-5 kHz, the pulse width is 75-150 ns, and the energy density is 3.3-5 J / cm 2 .
[0013] Furthermore, the semiconductor sample is a metal-SiC composite structure in which a metal layer is deposited on the surface of a SiC wafer, the material of the metal layer is at least one of Ni, Ti, Pt or W, and the thickness of the metal layer is 60 to 140 nm.
[0014] Furthermore, the large-size flat-top light is a rectangular flat-top light spot, and its size is 1100 μm to 1300 μm in length and 300 to 400 μm in width.
[0015] In addition, the present invention also provides a semiconductor ohmic contact processing system based on laser annealing, including a laser, a beam shaping component for shaping the laser into a flat-top light, and an annealing scanning component for carrying a semiconductor sample; the annealing scanning component includes a displacement platform and a processing chamber, and a plurality of blowing holes are provided on the side of the processing chamber opposite to the injection port, and the blowing holes are located above the semiconductor sample.
[0016] Furthermore, the blowing hole is inclined downward by 5 to 15 degrees.
[0017] Furthermore, an air suction hole is provided on one side of the sample inlet of the processing chamber.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The present invention adopts a large-size flat-top light as the laser annealing light source, which greatly reduces the number of light spot movements when annealing large-area semiconductor materials, thereby shortening the processing time and improving the processing efficiency; at the same time, a single-direction blowing mode is used to assist the laser annealing process, effectively solving the local unevenness of the scanning area caused by large-spot annealing, thereby improving the product processing quality.
[0020] (2) The present invention adopts a laser defocusing processing method. In the defocused state, the spatial distribution of the phase and amplitude of the light beam near the focus is more diffuse, so that the phase difference of the light beam at different positions is reduced, and the interference and diffraction effects become more uniform. When each sub-beam is recombined, the contrast between high-intensity points and low-intensity points is reduced, further improving the uniformity of the spot of large-size flat-top light, thereby obtaining an ohmic contact structure with uniform surface morphology.
[0021] The present invention will be further described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a structural schematic diagram of a semiconductor ohmic contact processing system based on laser annealing of the present invention;
[0023] Figure 2 This is a topographic image of a large-sized flat-top spot used in Example 1 of the present invention;
[0024] Figure 3 This is the topography of the small-sized shaped spot used in conventional silicon carbide laser annealing;
[0025] Figure 4 is a microscope image of the sample after annealing and scanning processing at the focal position in Example 1 of the present invention;
[0026] Figure 5 1 are microscope images of samples after annealing and scanning processing at different defocus amounts in Example 1 of the present invention; wherein (a) the defocus amount is 750 μm, (b) the defocus amount is 350 μm, (c) the defocus amount is 150 μm, and (d) the defocus amount is 50 μm;
[0027] Figure 6 This is the spot morphology at a defocus of 350μm and the microscope image of the sample after annealing and scanning processing;
[0028] Figure 7 This is a microscope image after annealing and scanning processing with different laser energy densities in Example 1 of the present invention;
[0029] Figure 8 is a schematic structural diagram of a processing chamber in Embodiment 2 of the present invention;
[0030] Fig. 9 It is a schematic diagram of the laser scanning path and the direction of the gas path in the processing chamber in Example 2 of the present invention.
[0031] Explanation of the accompanying drawings: 1. Laser; 2. Half-wave plate; 3. Polarization beam splitter; 4. Beam expander; 5. Microlens array; 6. Reflector; 7. Focusing mirror; 8. Semiconductor sample; 9. Displacement platform; 10. Processing chamber; 11. Blowing hole; 12. Suction hole. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In the description of the present invention, it should be understood that the terms "center", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0034] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, a conflicting connection or an integral connection; for ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances; in the description of the present invention, unless otherwise specified, "multiple" and "several" mean two or more.
[0035] Embodiment 1:
[0036] For the existing conventional silicon carbide laser annealing, Figure 3The small-sized spot shown in the figure has the problem of low processing efficiency when processing large-area materials. This embodiment provides a semiconductor ohmic contact processing method based on laser annealing. When laser annealing is performed on the surface of a semiconductor sample, a large-sized flat-top light is used as an annealing light source to emit to the surface of the semiconductor sample for annealing scanning processing. Since the spot size is large, each exposure can cover a larger area. In this way, when annealing a large-area material, the number of spot movements can be reduced, thereby shortening the processing time and improving production efficiency. Among them, the flat-top light spot emitted to the surface of the semiconductor sample can be but not limited to a rectangular flat-top spot, a circular flat-top spot, a square flat-top spot, etc. In this embodiment, a rectangular flat-top spot is taken as an example, and its size is 1100μm to 1300μm in length and 300 to 400μm in width. Figure 2 As shown, the rectangular flat-top spot size is 300 μm×1100 μm.
[0037] Specifically, in this embodiment, the semiconductor sample is taken as an example of 6-inch SiC, and its area S = π*R 2 =182cm 2 , at the same laser frequency, if the embodiment of this embodiment is used Figure 2 The large rectangular flat-top spot (size 300 μm × 1100 μm) shown in the figure only needs 6.7 × 10 4 If the light spot is used Figure 3 For the small shaped spot shown (size 60μm×60μm), 5×10 6 It is obvious that when the large-sized flat-top light spot of this embodiment is used for annealing, the processing efficiency can be greatly improved.
[0038] However, when a large spot size is used for annealing, there may be a local non-uniformity in the scanning area, e.g. Figure 4 As shown in the figure, the microscope image of the sample during processing at the focal position, the process parameters are a repetition frequency of 1kHz and an energy density of 4J / cm 2 , and it was found that there was a local unevenness in the scanning area. In addition, except for the first line, there were unevenness in the following lines, and they were all located below the light spot. After many experiments and analyses, the reason for the process problems in the annealing process using a large-size light spot is that after the large-size light spot is scanned, particles will be generated around it, thereby affecting the uniformity of the scanning process of the next line. Since there are no particles when processing the first line, only the first line has no unevenness. Based on this, in this embodiment, during the scanning annealing process using a large-size flat-top light spot, the surface of the semiconductor sample is blown in a single direction, and the blowing direction is the same as the stepping direction of the semiconductor sample, such as Fig. 9As shown, through this unidirectional blowing design, the dust particles generated during the processing can be blown to the scanned area without affecting the subsequent scanning process, thereby solving the adverse factors caused by large-size spot annealing and improving the product processing quality. The blowing gas is nitrogen or argon.
[0039] In some implementations, the semiconductor sample is a metal-SiC composite structure with a metal layer deposited on the surface of a SiC wafer, wherein the SiC wafer has a diameter of 6 inches or 8 inches and a thickness of 100 to 500 μm, the material of the metal layer is at least one of Ni, Ti, Pt or W, and the thickness of the metal layer is 60 to 140 nm.
[0040] Specifically, the silicon carbide sample preparation process of this embodiment is as follows: first, a SiC wafer is provided for cleaning. Since the surface of the polished SiC wafer is smooth and flat, only acetone organic solvent is needed to remove organic pollutants that may remain on the surface and effectively remove some water-insoluble organic substances. Then, it is rinsed with deionized water to remove the solvent and other soluble impurities on the surface, and then blown dry with nitrogen to ensure that no solvent residue is left on the surface. After that, a metal layer is deposited on the cleaned SiC wafer. The SiC wafer has two different crystal planes, the C plane and the Si plane. This embodiment chooses to deposit a metal layer on the C plane. The selected deposition method can be evaporation or sputtering. The metal layer formed by the latter has better density, so magnetron sputtering is used to deposit the metal layer. Optionally, in this embodiment, the metal to be deposited on the surface of the SiC wafer is Ni, but since the adhesion of metal Ni on SiC is poor, in order to improve the adhesion of Ni on SiC, before depositing the metal Ni, a 5nm layer of Ti can be deposited on the SiC as an adhesion layer, and then the target metal Ni with a thickness of 100nm is deposited to form the metal-SiC composite structure.
[0041] Optionally, since semiconductor materials have selective absorption characteristics for lasers, effective absorption will only occur when the laser wavelength matches its energy gap, that is, when the energy of the photon is greater than the bandgap width of the semiconductor, the laser can be effectively absorbed by the semiconductor material. Based on this, in this embodiment, when laser annealing is performed on silicon carbide materials, the laser center wavelength is selected to be 200-400nm, and the laser center wavelength is preferably 380-400nm. Furthermore, the laser repetition frequency is designed to be 1-5kHz, the pulse width is 75-150ns, and the energy density is 3.3-5J / cm 2 .
[0042] In the optimized implementation mode, the laser M of the annealing treatment is selected in this embodiment. 2 Factor greater than 10. M 2The factor defines the difference between the actual beam and the ideal Gaussian beam. It represents the ratio of the divergence angle of the actual beam to the divergence angle of the ideal Gaussian beam. Therefore, M 2 The smaller the factor, the closer the beam is to the ideal Gaussian beam and the better the coherence. Therefore, conventional laser processing uses M 2 However, in this embodiment, the laser needs to be shaped into a large-sized flat-top light through a microlens array. 2 The factor is small. When the laser passes through the microlens array with a periodic structure, strong interference will occur between the sub-beams, and the uniformity of the focused spot will decrease. Therefore, this embodiment selects M 2 When a larger laser is used as the annealing light source, due to its low coherence, the interference effect when the sub-beams are superimposed is weakened, which is more conducive to forming a uniform large-sized flat-top spot.
[0043] In an optimized implementation mode, when a large-size flat-top light is emitted to the surface of a semiconductor sample, the surface of the semiconductor sample is scanned in a defocused manner; specifically, the defocus amount of the defocused scanning is designed to be 50 to 1000 μm. Figure 4 From the microscope image of the silicon carbide sample after annealing and scanning at the focal position, it can be seen that there is an obvious grid-like shape in the annealed area. After analysis, the reason is that the laser is divided into many sub-beams during the process of being shaped into a flat top light by the microlens array. These sub-beams produce interference at the focal position, thus forming a grid-like distribution. Based on this, although this embodiment adopts M 2 When a larger laser is used as the annealing light source, the interference effect when the sub-beams are superimposed will be weakened accordingly. However, in order to further ensure that the interference effect is minimized, the present embodiment adopts a laser defocusing processing method rather than a traditional focal position processing method. In the defocused state, the spatial distribution of the phase and amplitude of the light beam near the focus is more diffuse, resulting in a reduction in the phase difference of the light beam at different positions, and the interference and diffraction effects become more uniform. Each sub-beam reduces the contrast between high-intensity points and low-intensity points when recombined. Therefore, the present embodiment adopts a defocusing method for processing, which can further improve the uniformity of the light spot of the large-size flat-top light, thereby obtaining an ohmic contact structure with uniform surface morphology.
[0044] Specifically, this embodiment investigates the effect of different defocusing amounts on sample quality. Taking silicon carbide as an example, the same laser parameters are maintained, the defocusing amount is changed, and the surface morphology of the sample processed with different defocusing amounts is observed using an optical microscope. The results are as follows: Figure 5 As shown, (a) the defocus amount is 750μm, (b) the defocus amount is 350μm, (c) the defocus amount is 150μm, and (d) the defocus amount is 50μm. Figure 4 and Figure 5By comparison, it can be seen that compared with the focus processing method, the sample annealing morphology obtained by defocusing processing is more uniform, and Figure 5 It can be seen that when the defocus amount is 350 μm, the spot size and uniformity are both better. Therefore, in this embodiment, the defocus amount of the laser annealing process is preferably 350 μm.
[0045] Based on the above analysis, the defocus is fixed at 350 μm, and the laser annealing process parameters are set: a UV laser with a central wavelength of 351 nm, a repetition frequency of 1 kHz, and an energy density of 4 J / cm 2 , Laser M 2 The factor is 12, and multiple lines are printed continuously. The morphology after annealing is observed under a microscope. The results are as follows Figure 6 As shown. Figure 6 It can be seen that the surface morphology of the sample after annealing is uniform and there is no obvious gridding phenomenon.
[0046] In addition, this example also investigates the effect of different laser energy density processing on sample quality. The defocus is fixed at 350 μm, the energy density is changed, and the surface morphology of the sample processed with different energy densities is observed using an optical microscope. The results are as follows: Figure 7 As shown, (a) energy density 3.3J / cm 2 (b) Energy density 3.6 J / cm 2 (c) Energy density 3.9 J / cm 2 (d) Energy density 5.0 J / cm 2 (e) Energy density 2.7 J / cm 2 (f) Energy density 5.5 J / cm 2 .Depend on Figure 7 It can be seen that when the energy density is too high or too low, the surface morphology of the sample after annealing is very uneven, while the energy density is between 3.3 and 5 J / cm 2 Within the range, the surface morphology of the samples after annealing is very uniform and flat, without obvious gridding phenomenon.
[0047] Embodiment 2:
[0048] like Figure 1 and Figure 8 As shown, this embodiment provides a semiconductor ohmic contact processing system based on laser annealing, including a laser 1, a beam shaping component for shaping the laser into a flat-top light, and an annealing scanning component for carrying a semiconductor sample 8; the annealing scanning component includes a displacement platform 9 and a processing chamber 10, and the two are linked to drive the semiconductor sample 8 to move two-dimensionally in the X and Y directions to adjust the position of the area to be scanned of the semiconductor sample 8, and a plurality of blowing holes 11 are provided on the side of the processing chamber 10 opposite to the injection port, and the blowing holes 11 are located above the semiconductor sample 8.
[0049] In an optional embodiment, the beam shaping component includes a half-wave plate 2, a polarization beam splitter prism 3, a beam expander 4, a microlens array 5, a reflector 6 and a focusing mirror 7, which are used to modulate and shape the laser emitted by the laser 1 into a large-sized flat-top light.
[0050] In some embodiments, the half-wave plate 2 is installed on a rotating motor, which controls the rotation angle of the half-wave plate 2 and forms a power attenuator with the polarization beam splitter prism 3 to jointly control the laser power. After calibrating the power value corresponding to the angle of the rotating motor, a specific rotation angle can be set to obtain the required laser power value, thereby realizing continuous adjustment of the laser power during processing.
[0051] In the optimized implementation mode, a blowing hole 11 is provided on one side of the processing chamber 10, and the blowing hole 11 is arranged to be tilted downward by 5 to 15 degrees, so as to form a better blowing effect on the surface of the sample to be processed, and to blow the particles on the surface of the sample to the scanned area. Furthermore, an air suction hole 12 is provided on one side of the sample inlet of the processing chamber 10, that is, an air suction hole 12 is provided on the opposite side of the air blowing hole 11, and air is sucked on the opposite side while blowing, so that the particles on the surface of the sample are blown to the scanned area faster.
[0052] For further optimization, when manufacturing semiconductor ohmic contacts by laser annealing, it is necessary to eliminate the interference of oxygen, and generally the oxygen content needs to be less than 10 ppm. Therefore, in this embodiment, a precise oxygen content analyzer is configured in the processing chamber 10 to detect the oxygen content in the chamber during processing.
[0053] In order to obtain the laser power value used in laser annealing, a power detector is further configured in the processing chamber 10, and the height of the power detector is consistent with the height of the semiconductor sample placed in the processing chamber 10. This can eliminate the effect of the protective glass of the processing chamber 10 on laser attenuation, so that the actual power incident on the semiconductor sample during processing can be detected to obtain a more accurate power value.
[0054] In summary, the present invention adopts a large-size flat-top light as the annealing light source, and rationally designs the chamber blowing direction and processing method of the processing system, forming a unidirectional blowing-assisted defocused laser processing strategy, which not only improves the annealing efficiency, but also solves the adverse effects of large spot processing, and obtains an ohmic contact structure with uniform surface morphology.
[0055] The above examples are merely illustrative of the present invention and do not constitute a limitation on the protection scope of the present invention. All designs that are the same or similar to the present invention fall within the protection scope of the present invention.
Claims
1. A semiconductor ohmic contact processing method based on laser annealing, characterized in that: When laser annealing is performed on the surface of a semiconductor sample, a large-size flat-top light is used as the annealing light source to be emitted to the surface of the semiconductor sample, and air is blown in a single direction on the surface of the semiconductor sample, and the blowing direction is the same as the stepping direction of the semiconductor sample.
2. The semiconductor ohmic contact processing method based on laser annealing according to claim 1, characterized in that: When the large-size flat-top light is emitted to the surface of the semiconductor sample, the surface of the silicon carbide sample is scanned in a defocused manner.
3. The semiconductor ohmic contact processing method based on laser annealing according to claim 2, characterized in that: The defocus amount of the defocus scanning method is 50 to 1000 μm.
4. The semiconductor ohmic contact processing method based on laser annealing according to any one of claims 1 to 3, characterized in that: The laser M of the laser annealing process 2 The factor is greater than 10.
5. The semiconductor ohmic contact processing method based on laser annealing according to any one of claims 1 to 3, characterized in that: The laser center wavelength of the laser annealing treatment is 200-400nm, the repetition frequency is 1-5kHz, the pulse width is 75-150ns, and the energy density is 3.3-5J / cm 2 .
6. The semiconductor ohmic contact processing method based on laser annealing according to any one of claims 1 to 3, characterized in that: The semiconductor sample is a metal-SiC composite structure with a metal layer deposited on the surface of a SiC wafer, the material of the metal layer is at least one of Ni, Ti, Pt or W, and the thickness of the metal layer is 60 to 140 nm.
7. The semiconductor ohmic contact processing method based on laser annealing according to any one of claims 1 to 3, characterized in that: The large-size flat-top light is a rectangular flat-top light spot, and its size is 1100 μm to 1300 μm in length and 300 to 400 μm in width.
8. A semiconductor ohmic contact processing system based on laser annealing, characterized in that: The semiconductor ohmic contact processing method used in any one of claims 1 to 7 comprises a laser, a beam shaping component for shaping the laser into a flat-top light, and an annealing scanning component for carrying a semiconductor sample; the annealing scanning component comprises a displacement platform and a processing chamber, a plurality of blowing holes are provided on a side of the processing chamber opposite to the injection port, and the blowing holes are located above the semiconductor sample.
9. The semiconductor ohmic contact processing system based on laser annealing as claimed in claim 8, characterized in that: The blowing hole is inclined downward by 5 to 15 degrees.
10. The semiconductor ohmic contact processing system based on laser annealing as claimed in claim 8, characterized in that: An air suction hole is arranged on one side of the sample inlet of the processing chamber.