Preparation method of semiconductor structure

By forming a melt bond between the hydrogen-containing release layer and the second bonding layer on the semiconductor substrate, the layout density and electrical performance problems caused by the thickness deviation of the bonding layer are solved, and higher yield and cost savings are achieved.

CN119008423AActive Publication Date: 2024-11-22CHANGXIN MEMORY TECH INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310553961.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-22
Estimated Expiration
2043-05-15

AI Technical Summary

Technical Problem

During semiconductor manufacturing, the large deviation of the total thickness of the bonding layer leads to uneven line width and spacing of the semiconductor device, reducing layout density and electrical properties, and easily damage the device during debonding and reducing yield.

Method used

By forming a first bonding layer on the first surface of the semiconductor substrate, and injecting hydrogen ions into the substrate to form a hydrogen-containing stripping layer, the second bonding layer combined with the carrier is melt bonded to reduce the total thickness deviation, and The peeling layer is separated from the substrate by heat treatment, avoiding local high temperatures caused by laser debonding.

Benefits of technology

It improves the layout density and electrical performance of semiconductor devices, avoids device damage, improves yield, and realizes the recycling of carriers through chemical mechanical grinding processes, reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008423A_ABST
    Figure CN119008423A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a preparation method of a semiconductor structure, and the method comprises the steps: providing a substrate which is provided with a first surface and a second surface which are opposite to each other; forming a first bonding layer on the first surface; injecting hydrogen ions into the substrate at one side of the first surface so as to form a hydrogen-containing stripping layer in the substrate; providing a carrier, and forming a second bonding layer on the surface of one side of the carrier; carrying out fusion bonding on the first bonding layer and the second bonding layer; forming a semiconductor device on the second surface of the substrate; and the stripping layer is processed, so that the stripping layer is separated from the substrate. According to the preparation method disclosed by the embodiment of the invention, the layout density of the semiconductor device can be improved, the electrical performance of the semiconductor device is improved, the semiconductor device is prevented from being damaged during de-bonding, and the yield of the semiconductor structure is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of semiconductor manufacturing technology, and in particular to a method for manufacturing a semiconductor structure. Background Art

[0002] During the semiconductor manufacturing process, various semiconductor devices are prepared on the front side of the semiconductor substrate. At this time, the back side of the semiconductor substrate needs to be temporarily bonded to the glass. During bonding, an adhesive layer is required to bond the back side of the semiconductor substrate to the glass. However, after using the adhesive layer, due to the large total thickness variation (Total Thickness Variation, TTV) of the adhesive layer, when preparing semiconductor devices on the front side of the semiconductor, the line width and spacing are large, which reduces the layout density and the electrical performance of the semiconductor structure. Moreover, when debonding, the semiconductor device is easily damaged, which reduces the yield of the semiconductor structure.

[0003] The above information disclosed in this background section is only for enhancement of understanding of the background of the present disclosure and therefore it may include information that does not constitute the relevant technology that is already known to one of ordinary skill in the art. Summary of the invention

[0004] The embodiments of the present disclosure provide a method for preparing a semiconductor structure, which can improve the layout density of semiconductor devices and improve the electrical performance and yield of semiconductor devices.

[0005] An embodiment of the present disclosure provides a method for preparing a semiconductor structure, comprising: providing a substrate, the substrate having a first surface and a second surface relative to each other; forming a first bonding layer on the first surface; injecting hydrogen ions into the substrate on one side of the first surface to form a hydrogen-containing peeling layer in the substrate; providing a carrier and forming a second bonding layer on a surface of one side of the carrier; melt-bonding the first bonding layer and the second bonding layer; forming a semiconductor device on the second surface of the substrate; and processing the peeling layer to separate the peeling layer from the substrate.

[0006] In some embodiments of the present disclosure, the peeling layer is processed to separate the peeling layer from the substrate, including: heat treating the substrate on which the semiconductor device is formed and the carrier to separate the peeling layer from the substrate, so as to separate the carrier from the substrate.

[0007] In some embodiments of the present disclosure, the temperature of heat treating the substrate on which the semiconductor device is formed and the carrier is 300° C. to 450° C.

[0008] In some embodiments of the present disclosure, melt-bonding the first bonding layer and the second bonding layer includes: laminating the first bonding layer and the second bonding layer at room temperature and pressure; and annealing at a temperature below 250° C. to melt-bond the first bonding layer and the second bonding layer.

[0009] In some embodiments of the present disclosure, the method further includes: after the release layer is separated from the substrate, removing the first bonding layer on the second bonding layer and residual material of the substrate using a chemical mechanical polishing process.

[0010] In some embodiments of the present disclosure, the material of the first bonding layer includes silicon oxide; and / or the material of the second bonding layer includes at least one of silicon oxide, silicon carbonitride and silicon nitride.

[0011] In some embodiments of the present disclosure, the thickness of the first bonding layer is 0.8-1.2 μm.

[0012] In some embodiments of the present disclosure, the thickness of the second bonding layer is 0.1-1 μm.

[0013] In some embodiments of the present disclosure, in the vertical direction, the depth of the hydrogen ions implanted into the substrate is 1-5 μm.

[0014] In some embodiments of the present disclosure, the amount of hydrogen ions implanted is 2×10 16 ~1×10 17 Pieces / cm 2 .

[0015] In some embodiments of the present disclosure, the material of the carrier is the same as that of the substrate; or, the material of the carrier is glass.

[0016] It can be seen from the above technical solutions that the method for preparing the semiconductor structure of the embodiment of the present disclosure has at least one of the following advantages and positive effects:

[0017] In the disclosed embodiment, a first bonding layer is formed on the first surface of the substrate, a second bonding layer is formed on the surface of one side of the carrier, and the first bonding layer and the second bonding layer are melt-bonded, so that the total thickness deviation of the first bonding layer and the second bonding layer after bonding is reduced, so that when a semiconductor device is formed on the second surface of the substrate, the layout density of the semiconductor device can be improved, thereby improving the electrical performance of the semiconductor structure. In addition, by injecting hydrogen ions into the substrate to form a hydrogen-containing peeling layer, the debonding of the substrate and the carrier is made easier, thereby avoiding damage to the semiconductor device and improving the yield of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The above and other features and advantages of the present disclosure will become more apparent by describing in detail example embodiments thereof with reference to the attached drawings.

[0019] Figure 1 A flow chart of a method for preparing a semiconductor structure according to some embodiments of the present disclosure;

[0020] Figure 2 A schematic diagram of a substrate according to some embodiments of the present disclosure;

[0021] Figure 3 A schematic diagram of forming a first bonding layer on a substrate according to some embodiments of the present disclosure;

[0022] Figure 4 A schematic diagram of injecting hydrogen ions into a substrate according to some embodiments of the present disclosure;

[0023] Figure 5 A schematic diagram of a carrier according to some embodiments of the present disclosure;

[0024] Figure 6 A schematic diagram of forming a second bonding layer on a carrier according to some embodiments of the present disclosure;

[0025] Figure 7 A schematic diagram of melt-bonding a first bonding layer and a second bonding layer according to some embodiments of the present disclosure;

[0026] Figure 8 A schematic diagram showing a semiconductor device formed on the second surface of a substrate according to some embodiments of the present disclosure;

[0027] Fig. 9 A schematic diagram showing separation of a substrate and a carrier according to some embodiments of the present disclosure;

[0028] Fig.10 Schematic diagram of chemical mechanical polishing of a separated carrier according to some embodiments of the present disclosure.

[0029] Description of reference numerals:

[0030] 1. Substrate; 11. First surface; 12. Second surface; 2. First bonding layer; 3. Stripping layer; 4. Carrier; 5. Second bonding layer; 6. Semiconductor device; 7. Insulating layer; 100. Grinding head; Y, vertical direction. DETAILED DESCRIPTION

[0031] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided so that this disclosure will be comprehensive and complete and will fully convey the concepts of the example embodiments to those skilled in the art. The same reference numerals in the figures represent the same or similar structures, and thus their detailed description will be omitted.

[0032] In the following description of different exemplary embodiments of the present disclosure, reference is made to the accompanying drawings, which form a part of the present disclosure and in which different exemplary structures that can implement multiple aspects of the present disclosure are shown by way of example. It should be understood that other specific schemes of components, structures, exemplary devices, systems and steps can be used, and structural and functional modifications can be made without departing from the scope of the present disclosure. Moreover, although the terms "above", "between", "within", etc. may be used in this specification to describe different exemplary features and elements of the present disclosure, these terms are used herein only for convenience, such as according to the direction of the examples in the accompanying drawings. Nothing in this specification should be construed as requiring a specific three-dimensional direction of the structure to fall within the scope of the present disclosure. In addition, the terms "first", "second", etc. in the claims are used only as marks and are not numerical limitations on their objects.

[0033] The flowcharts shown in the accompanying drawings are only exemplary and do not necessarily include all the contents and operations / steps, nor must they be executed in the order described. For example, some operations / steps can be decomposed, and some operations / steps can be combined or partially combined, so the actual execution order may change according to actual conditions.

[0034] In addition, in the description of the present disclosure, “plurality” means at least two, for example, two, three, etc., unless otherwise clearly and specifically defined.

[0035] In the process of semiconductor manufacturing, various semiconductor devices, such as RDL (Re-distribution layer) or other devices, are prepared on the front side of the semiconductor substrate. At this time, the back side of the semiconductor substrate needs to be temporarily bonded to the glass. During temporary bonding, an adhesive layer and a release layer are sequentially formed on the back side of the semiconductor substrate. The adhesive layer is bonded to the back side of the semiconductor substrate, and the release layer is bonded to the adhesive layer and the surface of the glass, thereby achieving temporary bonding between the semiconductor substrate and the glass.

[0036] However, the study found that due to the relatively thick thickness of the bonding layer, which is generally tens of microns, the total thickness deviation is relatively large, reaching the micron level, for example, 5 microns. The total thickness deviation can be understood as the distribution of surface thickness, that is, the difference between the maximum thickness value and the minimum thickness value in multiple thickness measurements. Therefore, the surface of the bonding layer appears uneven. In this way, when the semiconductor substrate is temporarily bonded to the glass and a semiconductor device is prepared on the front side of the semiconductor substrate, it will be greatly affected, resulting in larger feature sizes and spacing of the semiconductor device, reducing the layout density, and thus reducing the electrical performance of the semiconductor structure.

[0037] In addition, since it is a temporary bond, after the semiconductor device is prepared, the semiconductor substrate and the glass need to be debonded. That is, the semiconductor substrate is irradiated with a laser to generate a local high temperature, so that the release layer is carbonized, thereby achieving debonding. However, the local high temperature generated by laser irradiation may be transmitted to the semiconductor device, affecting the performance of the semiconductor device and reducing the yield. Moreover, after debonding, the glass loses its use value, and the glass needs to be replaced during the next bonding, resulting in high costs.

[0038] Based on this, the present disclosure provides a method for preparing a semiconductor structure. Figures 1 to 10 As shown, Figure 1 is a flow chart of the preparation method of the embodiment of the present disclosure, Figures 2 to 10 FIG. 1 is a schematic diagram of the structure of a semiconductor structure at different steps in the preparation method. Figure 1 As shown, the method includes the following steps S110 to S170.

[0039] S110 : providing a substrate 1 , wherein the substrate 1 has a first surface 11 and a second surface 12 opposite to each other.

[0040] S120 : forming a first bonding layer 2 on the first surface 11 .

[0041] S130 : On one side of the first surface 11 , hydrogen ions are implanted into the substrate 1 to form a hydrogen-containing peeling layer 3 in the substrate 1 .

[0042] S140 : providing a carrier 4 , and forming a second bonding layer 5 on a surface of one side of the carrier 4 .

[0043] S150: melt-bonding the first bonding layer 2 and the second bonding layer 5.

[0044] S160 : forming a semiconductor device 6 on the second surface 12 of the substrate 1 .

[0045] S170 : The peeling layer 3 is processed to separate the peeling layer 3 from the substrate 1 .

[0046] In the disclosed embodiment, a first bonding layer 2 is formed on the first surface 11 of the substrate 1, a second bonding layer 5 is formed on the surface of one side of the carrier 4, and the first bonding layer 2 and the second bonding layer 5 are melt-bonded, so that the total thickness deviation of the first bonding layer 2 and the second bonding layer 5 after bonding is reduced, so that when the semiconductor device 6 is formed on the second surface 12 of the substrate 1, the layout density of the semiconductor device 6 can be improved, thereby improving the electrical performance of the semiconductor structure. In addition, by injecting hydrogen ions into the substrate to form a hydrogen-containing peeling layer, the debonding of the substrate and the carrier is easier, avoiding damage to the semiconductor device and improving the yield of the semiconductor structure.

[0047] The following is a detailed description of the method for preparing the semiconductor structure according to the embodiment of the present disclosure.

[0048] S110 : providing a substrate 1 , wherein the substrate 1 has a first surface 11 and a second surface 12 opposite to each other.

[0049] like Figure 1 and Figure 2 As shown, a substrate 1 is provided, and the material of the substrate 1 can be silicon, silicon carbide, silicon on insulator, stacked silicon on insulator, stacked silicon germanium on insulator, silicon germanium on insulator or germanium on insulator. Shallow trench isolation can be formed in the substrate 1, and active areas are provided between the shallow trench isolations. For ease of explanation, Figure 2 The above structure is not shown in the substrate 1 in FIG.

[0050] In the vertical direction Y, the substrate 1 has a first surface 11 and a second surface 12 opposite to each other. The vertical direction Y is a direction perpendicular to the substrate 1. The first surface 11 of the substrate 1 is used for temporary bonding. The second surface 12 may be provided with an active area and a device area.

[0051] S120 : forming a first bonding layer 2 on the first surface 11 .

[0052] like Figure 3 As shown, a deposition process may be used to form a first bonding layer 2 on the first surface 11 of the substrate 1. The material of the first bonding layer 2 may include silicon oxide (SiO2).

[0053] In some embodiments, silicon oxide may be formed on the first surface 11 of the substrate 1 by a deposition process. The deposition process may include a chemical vapor deposition process, a physical vapor deposition process, an atomic layer deposition process, etc., which are not particularly limited here.

[0054] In some embodiments, when the material of the substrate 1 is Si, a silicon oxide layer can also be formed on the Si surface by thermal oxidation process as the first bonding layer 2, and the thickness of the formed silicon oxide can be controlled by controlling the concentration, dosage, temperature and other parameters of oxygen. No matter what process is used, as long as the first bonding layer 2 can be formed, the specific process is not limited here.

[0055] In some embodiments, the thickness of the first bonding layer 2 may be 0.8 to 1.2 μm. Specifically, in addition to the above two end values, the thickness of the first bonding layer 2 may also be 0.9 μm, 1 μm, 1.05 μm, 1.1 μm, or 1.15 μm, which is not specifically limited here. The thickness of the first bonding layer 2 is the dimension of the first bonding layer 2 in the vertical direction Y.

[0056] In the disclosed embodiment, the material of the first bonding layer 2 is SiO2, and the crystal structure of SiO2 is a regular tetrahedron. The silicon atom is located at the center of the regular tetrahedron, and the four oxygen atoms are located at the four vertices of the regular tetrahedron. Many such tetrahedrons are connected by the oxygen atoms at the vertices, and each oxygen atom is shared by two tetrahedrons. The regular tetrahedron crystal structure of SiO2 is conducive to the injection of hydrogen ions in the subsequent process and improves the uniformity of the injection. In addition, setting the thickness of the first bonding layer 2 to 0.8 to 1.2 μm can further facilitate the injection of hydrogen ions.

[0057] S130 : On one side of the first surface 11 , hydrogen ions are implanted into the substrate 1 to form a hydrogen-containing peeling layer 3 in the substrate 1 .

[0058] like Figure 4 As shown, an ion implantation process can be used to implant hydrogen ions (H + ). Specifically, the substrate 1 is irradiated with a hydrogen ion beam, and the hydrogen ions are injected into the substrate 1 through the first bonding layer 2. The hydrogen ions are slowly decelerated by the resistance of the solid material of the substrate 1, so that the hydrogen ions finally stay in the substrate 1 and are located at a certain depth. The hydrogen ions are injected into the substrate 1 through the first bonding layer 2. Since the first bonding layer 2 is a silicon oxide crystal with a regular tetrahedral structure, the hydrogen ions are more easily injected into the substrate 1. In the vertical direction Y, the depth of the hydrogen ions injected into the substrate 1 is 1 to 5 μm.

[0059] like Figure 4As shown, the depth of the substrate 1 can be understood as the distance extending from the first surface 11 of the substrate 1 to the second surface 12 in the vertical direction Y. Due to process reasons, the hydrogen ions are not injected into the first surface 11. In the vertical direction Y, after extending a certain distance from the first surface 11 to the second surface 12, the hydrogen ions begin to be injected into the substrate 1 and disperse to a certain depth in the direction close to the second surface 12 to form the peeling layer 3.

[0060] In some embodiments, in addition to the two end values ​​mentioned above, the depth of hydrogen ion implantation into the substrate 1 can also be 2μm, 2.5μm, 3μm, 3.5μm, 4μm, or 4.5μm. The depth of hydrogen ion implantation into the substrate 1 can be adjusted according to the size of the substrate 1 and process requirements, and is not specifically limited here.

[0061] In some embodiments, the depth of hydrogen ion implantation into the substrate 1 can be controlled by adjusting parameters such as the speed and temperature of ion implantation.

[0062] After the hydrogen ions are injected, micro cavities can be formed in the stripping layer 3, that is, after the hydrogen ions are injected, bubbles can be formed inside the substrate 1. In other words, the stripping layer 3 contains bubbles, and the substrate 1 is heat treated in the subsequent process, which can increase the pressure of the bubbles and penetrate the entire micro cavity, thereby realizing the separation of the stripping layer 3 and the substrate 1.

[0063] In some embodiments, the amount of hydrogen ions implanted is 2×10 16 ~1×10 17 Pieces / cm 2 (ions / cm 2 Specifically, in addition to the above two end values, the amount of hydrogen ion implantation can also be 2×10 16 Pieces / cm 2 , 3×10 16 Pieces / cm 2 , 5×10 16 Pieces / cm 2 , 6×10 16 Pieces / cm 2 ,7×10 16 Pieces / cm 2 , 8×10 16 Pieces / cm 2 ,9×10 16 Pieces / cm 2 , no special limitation is made here.

[0064] The amount of hydrogen ion injection needs to be controlled within a certain range. If the amount of hydrogen ion injection is too large, hydrogen ion escape will occur, causing the substrate 1 to have hole-like defects, thereby affecting the preparation of the semiconductor structure and its electrical properties, and reducing the yield of the semiconductor structure; if the amount of hydrogen ion injection is too small, continuous bubbles cannot be formed inside the substrate 1, making it difficult to separate the peeling layer 3 from the substrate 1 during the subsequent heat treatment process. In the embodiment of the present disclosure, the amount of hydrogen ion injection is set to the above range (2×10 16 ~1×10 17 Pieces / cm 2 ), which can avoid causing hole-shaped defects in the substrate 1 and can make the peeling layer 3 easier to separate from the substrate 1 in the subsequent process.

[0065] S140 : providing a carrier 4 , and forming a second bonding layer 5 on a surface of one side of the carrier 4 .

[0066] like Figure 5 As shown, a carrier 4 is provided, and the carrier 4 is used to bond with the substrate 1. The material of the carrier 4 is the same as that of the substrate 1; or, the material of the carrier 4 is glass. In some embodiments, the material of the carrier 4 can also be the same as that of the semiconductor substrate 1, for example, the material of the carrier 4 can be silicon, silicon carbide, silicon on insulator, stacked silicon on insulator, stacked silicon germanium on insulator, silicon germanium on insulator, or germanium on insulator.

[0067] In some embodiments, the material of the carrier 4 may be different from that of the substrate 1 , for example, the material of the carrier 4 is glass, that is, as long as the second bonding layer 5 in the subsequent process can be formed on the carrier 4 , no special limitation is made here.

[0068] like Figure 6 As shown, a deposition process may be used to form the second bonding layer 5 on the surface of the carrier 4. The deposition process may be at least one of a chemical vapor deposition process, a physical vapor deposition process and an atomic layer deposition process, which is not particularly limited here.

[0069] In some embodiments, the thickness of the second bonding layer 5 can be 0.1 to 1 μm. Specifically, in addition to the above two end values, it can also be 0.2 μm, 0.4 μm, 0.5 μm, 0.7 μm, 0.8 μm, 0.9 μm, and no special limitation is made here. The thickness of the second bonding layer 5 is set to the above range, and after the first bonding layer 2 and the second bonding layer 5 are melt-bonded in the subsequent process, the thickness of the first bonding layer 2 and the second bonding layer 5 is thinner, thereby making the total thickness deviation smaller, which can improve the layout density when preparing the semiconductor device 6, thereby improving the electrical performance of the semiconductor structure.

[0070] In some embodiments, the material of the second bonding layer 5 may include at least one of silicon oxide (SiO 2 ), silicon carbonitride (SiNC) and silicon nitride (Si 3 N 4 ).

[0071] The material of the first bonding layer 2 is silicon oxide, which can facilitate the injection of hydrogen ions. Since the second bonding layer 5 needs to be melt-bonded with the first bonding layer 2 in the subsequent process, the material of the second bonding layer 5 can be at least one of the above-mentioned silicon oxide, silicon carbonitride and silicon nitride, all of which can be melt-bonded with silicon oxide in a relatively stable and uniform manner, so that the temporary bonding between the substrate 1 and the carrier 4 is more stable, and the total thickness deviation of the first bonding layer 2 and the second bonding layer 5 after melt bonding is smaller.

[0072] S150: melt-bonding the first bonding layer 2 and the second bonding layer 5.

[0073] like Figure 7 As shown, the first bonding layer 2 and the second bonding layer 5 are melt-bonded, including: laminating the first bonding layer 2 and the second bonding layer 5 at room temperature and pressure; annealing at a temperature below 250° C. to melt-bond the first bonding layer 2 and the second bonding layer 5.

[0074] Specifically, normal temperature and pressure can be understood as a temperature of 25°C and a pressure of one atmosphere. Of course, normal temperature is not strictly 25°C. Due to changes in the weather, the temperature may fluctuate. For example, a temperature fluctuation of + / -5°C is acceptable. Normal pressure is not strictly an atmosphere. Due to weather reasons, the air pressure may fluctuate within a certain range, which is feasible. In other words, when the first bonding layer 2 and the second bonding layer 5 are bonded for preliminary fusion, the first bonding layer 2 and the second bonding layer 5 are not heated or cooled or the pressure is changed, so that the two are directly bonded by van der Waals force or atomic force at normal temperature and pressure.

[0075] At room temperature and pressure, the first bonding layer 2 and the second bonding layer 5 are bonded together, and preliminary melt bonding occurs between the two. After that, they are annealed at a temperature below 250°C, and further melt bonding occurs between the first bonding layer 2 and the second bonding layer 5, so that the two can be bonded more stably.

[0076] The annealing temperature may be 100°C to 250°C. In addition to these two end values, the annealing temperature may also be 120°C, 140°C, 150°C, 160°C, 180°C, 200°C, 220°C, 240°C, and no special limitation is made here. The annealing treatment is actually heating the first bonding layer 2 and the second bonding layer 5 that are initially bonded to increase the molecular activity of the two and further promote the combination of the two, thereby making the bonding more stable.

[0077] S160 : forming a semiconductor device 6 on the second surface 12 of the substrate 1 .

[0078] like Figure 8 As shown, after the substrate 1 and the carrier 4 are temporarily bonded, a semiconductor device 6 can be prepared on the second surface 12 of the substrate 1. The semiconductor device 6 can be a word line structure, a bit line structure, a capacitor structure or other conductive connection structure, and an insulating layer 7 is formed between the semiconductor devices 6. Since the substrate 1 and the carrier 4 are bonded by melt bonding of the first bonding layer 2 and the second bonding layer 5, the total thickness deviation of the first bonding layer 2 and the second bonding layer 5 is small, and the total thickness deviation is less than 500nm, or even less than 5nm, and the flatness is good, so the characteristic size and spacing of the semiconductor device 6 formed on the second surface 12 of the substrate 1 are reduced, the layout density of the semiconductor device is increased, more semiconductor devices 6 can be prepared on the substrate 1, and the electrical performance of the semiconductor structure is improved.

[0079] S170 : The peeling layer 3 is processed to separate the peeling layer 3 from the substrate 1 .

[0080] like Fig. 9 As shown, processing the peeling layer 3 to separate the peeling layer 3 from the substrate 1 includes: heat-treating the substrate 1 formed with the semiconductor device 6 and the carrier 4 to separate the peeling layer 3 from the substrate 1 , so as to separate the carrier 4 from the substrate 1 .

[0081] Since bubbles are formed in the peeling layer 3, when the substrate 1 and the carrier 4 are heat treated, the bubble pressure increases, which can also be understood as the bubbles becoming larger, and a micro-cavity layer is formed inside the peeling layer 3. The micro-cavity layer gradually connects with the growth of multiple bubbles, causing the peeling layer 3 to fall off and separate from the substrate 1. This causes the carrier 4 to separate from the substrate 1, and this process is also called the debonding of the carrier 4 and the substrate 1. After the substrate 1 and the carrier 4 are separated, as shown in FIG. Fig. 9 As shown, the second bonding layer 5 and the first bonding layer 2 are located on the carrier 4 side, and the first bonding layer 2 , part of the remaining substrate 1 material, and even part of the remaining release layer 3 are attached to the second bonding layer 5 .

[0082] In some embodiments, the temperature of heat treatment for the substrate 1 and the carrier 4 formed with the semiconductor device 6 is 300° C. to 450° C. Specifically, the heat treatment may be an annealing process, and the temperature of the heat treatment may be 320° C., 350° C., 380° C., 400° C., 420° C., 430° C. in addition to the above two end values, as long as the peeling layer 3 can be separated from the substrate 1 smoothly, and no special limitation is made here.

[0083] The substrate 1 and the carrier 4 are heat-treated at a temperature that is neither too high nor too low. If the temperature is too high, the local bubble pressure may be too high, resulting in the local peeling of the peeling layer 3 prematurely, making the surface of the substrate 1 discontinuous after peeling; if the temperature is too low, the peeling effect cannot be achieved. Therefore, in the embodiment of the present disclosure, the temperature of the heat treatment is set to the above range, which can control the bubble pressure in the peeling layer 3 so that the peeling layer 3 can be peeled evenly. After the peeling layer 3 is peeled, the surface of the substrate 1 is continuous, avoiding damage to the surface of the substrate 1. The bubbles in the peeling layer 3 are all connected, so that the peeling layer 3 can be completely peeled off, ensuring the smoothness of the surface of the substrate 1. In addition, the separation of the peeling layer 3 and the substrate 1 by low-temperature annealing realizes the debonding of the carrier 4 and the substrate 1, which is more gentle and avoids the situation where the substrate 1 is irradiated with a laser to generate local high temperature, thereby avoiding damage to the semiconductor device 6 and increasing the yield of the semiconductor structure.

[0084] In some embodiments, the method for preparing the semiconductor structure may further include: after the release layer 3 is separated from the substrate 1 , removing the first bonding layer 2 on the second bonding layer 5 and the remaining material of the substrate 1 by using a chemical mechanical polishing process.

[0085] like Fig. 9 As shown, after the carrier 4 is separated from the substrate 1, in the vertical direction Y, the surface of the carrier 4 has a bonded second bonding layer 5 and a first bonding layer 2, and there is residual substrate 1 material on the surface of the first bonding layer 2, and there may even be a very small amount of hydrogen-containing stripping layer 3 above the substrate 1 material.

[0086] In order to realize the reuse of the carrier 4, a chemical mechanical polishing (CMP) process can be used to remove the very small amount of hydrogen-containing peeling layer 3, the residual substrate 1 material and the first bonding layer 2, and retain the flat second bonding layer 5. Therefore, the carrier 4 and the second bonding layer 5 thereon can be used for melt bonding with the next substrate, so that the carrier 4 can be recycled for multiple times. Compared with the need to replace a new glass carrier every time, it greatly saves costs and is more environmentally friendly.

[0087] Among them, the chemical mechanical polishing process is a process that combines the chemical reaction process with the mechanical polishing process. Fig.10As shown, during the grinding process, the grinding head 100 applies a certain pressure on the side of the carrier 4 that does not have the second bonding layer 5, so that the grinding surface of the carrier 4 (the surface on the second bonding layer 5) is tightly attached to the grinding pad. The grinding pad itself rotates, and at the same time, the grinding head 100 drives the carrier 4 to rotate in the same direction as the grinding pad. In this process, a grinding liquid is used, and the grinding liquid contains tiny grinding particles, so that the grinding surface of the carrier 4 and the surface of the grinding pad generate mechanical friction. During the grinding process, the hydrogen-containing peeling layer 3, the residual material of the substrate 1, and the first bonding layer 2 on the second bonding layer 5 are removed through a series of complex mechanical and chemical actions. When the surface of the second bonding layer 5 is ground, the grinding is stopped to achieve the purpose of removing the above-mentioned film layer and flattening, so that the carrier 4 with the second bonding layer 5 can be recycled for multiple times.

[0088] In summary, the preparation method of the embodiment of the present disclosure forms a first bonding layer 2 on the first surface 11 of the substrate 1, forms a second bonding layer 5 on the surface of one side of the carrier 4, and melt-bonds the first bonding layer 2 and the second bonding layer 5, so that the total thickness deviation of the first bonding layer 2 and the second bonding layer 5 after bonding is reduced, so that when the semiconductor device 6 is formed on the second surface 12 of the substrate 1, the layout density of the semiconductor device 6 can be improved, thereby improving the electrical performance of the semiconductor structure. In addition, the separation of the peeling layer 3 and the substrate 1 is used to achieve the debonding of the carrier 4 and the substrate 1, which is a more gentle means, avoiding the situation where the substrate 1 is irradiated with a laser to generate local high temperature, thereby avoiding damage to the semiconductor device 6, and increasing the yield of the semiconductor structure. The surface of the carrier 4 is ground using a chemical mechanical grinding process, so that the carrier 4 can be reused. Compared with the need to replace a new glass carrier every time, it greatly saves costs and is more environmentally friendly.

[0089] The disclosed embodiment also provides a semiconductor structure, which may be, for example, a DRAM (Dynamic Random Access Memory), an SRAM (Static Random Access Memory) or a ROM (Read Only Memory), and the semiconductor structure may be prepared using the method described in any of the above embodiments, thereby increasing the layout density of the semiconductor structure, improving the electrical performance and yield of the semiconductor, and saving costs. For the specific steps of the preparation method, reference may be made to the description of any of the above embodiments, and no further description will be given here.

[0090] It should be understood that the present disclosure does not limit its application to the detailed structure and arrangement of the components proposed in this specification. The present disclosure can have other embodiments and can be implemented and executed in a variety of ways. The aforementioned variations and modifications fall within the scope of the present disclosure. It should be understood that the present disclosure disclosed and defined in this specification extends to all alternative combinations of two or more individual features mentioned or evident in the text and / or the drawings. All these different combinations constitute multiple alternative aspects of the present disclosure. The embodiments described in this specification illustrate the best mode known for implementing the present disclosure and will enable those skilled in the art to adopt the present disclosure.

Claims

1. A method for preparing a semiconductor structure, characterized in that: include: providing a substrate having a first surface and a second surface opposite to each other; forming a first bonding layer on the first surface; On one side of the first surface, injecting hydrogen ions into the substrate to form a hydrogen-containing peeling layer in the substrate; Providing a carrier, and forming a second bonding layer on a surface of one side of the carrier; melt-bonding the first bonding layer and the second bonding layer; forming a semiconductor device on the second surface of the substrate; The release layer is processed to separate the release layer from the substrate.

2. The method according to claim 1, characterized in that The peeling layer is processed to separate the peeling layer from the substrate, comprising: The substrate on which the semiconductor device is formed and the carrier are subjected to a heat treatment to separate the peeling layer from the substrate, thereby separating the carrier from the substrate.

3. The method according to claim 2, characterized in that The temperature of heat treating the substrate on which the semiconductor device is formed and the carrier is 300° C. to 450° C.

4. The method according to claim 1, characterized in that: The first bonding layer and the second bonding layer are melt-bonded, comprising: Laminating the first bonding layer and the second bonding layer at room temperature and pressure; Annealing is performed at a temperature lower than 250° C. to melt-bond the first bonding layer and the second bonding layer.

5. The method according to any one of claims 1 to 4, characterized in that Also includes: After the peeling layer is separated from the substrate, the first bonding layer and the remaining material of the substrate on the second bonding layer are removed by a chemical mechanical polishing process.

6. The method according to any one of claims 1 to 4, characterized in that The material of the first bonding layer includes silicon oxide; and / or the material of the second bonding layer includes at least one of silicon oxide, silicon carbonitride and silicon nitride.

7. The method according to claim 1, characterized in that The thickness of the first bonding layer is 0.8-1.2 μm.

8. The method according to claim 1, characterized in that The thickness of the second bonding layer is 0.1-1 μm.

9. The method according to claim 1, characterized in that: In the vertical direction, the depth of the hydrogen ions implanted into the substrate is 1 to 5 μm.

10. The method according to claim 1, characterized in that The amount of hydrogen ions implanted is 2×10 16 ~1×10 17 Pieces / cm 2 .

11. The method according to claim 1, characterized in that: The material of the carrier is the same as that of the substrate; or, the material of the carrier is glass.

Citation Information

Patent Citations

  • Composite wafer for fabrication of semiconductor devices

    CN103165625A

  • Method for separating semiconductor substrate body from functional layer thereon

    CN108140608A

  • Bonding material, preparation method and semiconductor device

    CN114975096A

  • Semiconductor structure and method for manufacturing the same

    US20170084479A1

  • Trim free wafer bonding methods and devices

    US20230142902A1