Salt-mist-resistant parallel seam welding packaging structure and preparation method thereof
By using high-purity nickel protective layer and electroless nickel-plated phosphorus alloy solder layer in parallel seam welding packages, combined with annealing treatment, the corrosion problem of parallel seam welding packages in salt spray tests is solved, achieving efficient salt spray resistance and cost reduction effect.
Patent Information
- Application Number
- CN202411081429.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
The existing parallel seam welded packaging is prone to corrosion in salt spray test, resulting in failure of the sealing of the packaging structure, and the salt spray resistance process is high and the effect on high temperatures is poor.
The ceramic or metal encapsulation shell is combined with the alloy cover plate. The surface of the alloy cover plate is covered with a high-purity nickel protective layer and an electroless nickel-phosphorus alloy solder layer. The nickel-phosphorus alloy melting point of the solder layer is less than 900℃, and nickel is formed by electroplating and electroless plating. Phosphorus alloy solder layer, combined with annealing treatment to enhance connection strength.
It realizes the connection between the cover plate and the tube and shell, reduces the packaging cost, improves the corrosion resistance of salt spray, and is compatible with the existing parallel seam welding process.
Smart Images

Figure CN119008535A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electronic packaging, and in particular to a salt-fog resistant parallel seam welding packaging structure and a preparation method thereof. Background Art
[0002] Parallel seam welding is mainly used in the field of electronic packaging, especially in the packaging of small precision components such as integrated circuits and semiconductor devices. The principle of parallel seam welding is to apply pressure and pulse current on the surface of the parts to be welded through two electrode rollers. The current generates high temperature at the contact resistance position between the electrode and the cover plate, and the cover plate and the tube shell, so that the cover plate coating melts and becomes a welding point between the cover plate and the tube shell. With the slow rolling of the electrode wheel and the action of continuous pulse discharge, the welding points are connected into a line to form a complete welding between the cover plate and the tube shell, isolating the inside and outside of the cavity to protect the internal electrical structure. This process has the advantages of low overall temperature rise, high reliability and low cost.
[0003] Conventional parallel seam welded cover plates are usually made of Kovar alloy or iron-nickel alloy, which is composed of iron, nickel and other elements. When used, due to the low standard electrode potential of iron element and poor corrosion resistance, a nickel-gold composite coating or a composite nickel layer needs to be plated on the surface as a protective layer.
[0004] After the parallel seam welding package, the coating in the welding line area is melted by high temperature and leaks out the substrate below. In the salt spray test, the metals with different standard potentials exposed to the outside will form a galvanic system, which will quickly corrode to form rust spots, and cause the sealing failure of the packaging structure over time. At the same time, for circuits with salt spray corrosion resistance requirements, gold-tin alloy solder sealing process is usually used, but this process will greatly increase the packaging cost of the circuit, and the process is less effective for packaging structures that are not resistant to high temperatures. Therefore, a salt spray-resistant parallel seam welding packaging structure and a preparation method thereof are proposed. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a salt-fog resistant parallel seam welding packaging structure and a preparation method thereof which has a salt-fog resistant effect, can reduce the packaging cost of a circuit, and improve the packaging effect of a circuit, and has practicality and wide application.
[0006] To solve the above problems, the present invention adopts the following technical solutions:
[0007] A salt spray resistant parallel seam welding packaging structure comprises two parts: a ceramic or metal packaging shell and an alloy cover plate; the base material of the alloy cover plate is Kovar or an iron-nickel alloy, and the thickness of the sealing area where the alloy cover plate is located is 0.08-0.1 mm; the surface of the alloy cover plate is covered with a protective layer, which is high-purity nickel formed by electroplating, has a melting point of 1455°C, and a thickness of 2μm-8.9μm; the outermost surface of the sealing area of the shell is covered with a solder layer; the solder layer is formed by chemical nickel plating, and the weight ratio of phosphorus in the nickel-phosphorus alloy is 8%-12%, and the melting point of the nickel-phosphorus alloy is lower than 900°C.
[0008] Preferably, the solder layer has a thickness of 2 to 5 μm.
[0009] Preferably, the thickness of the sealing area of the alloy cover plate is 0.08 mm.
[0010] Preferably, the weight ratio of phosphorus in the nickel-phosphorus alloy is 10%.
[0011] Preferably, the melting point of the nickel-phosphorus alloy is 880°C.
[0012] A method for preparing a salt spray resistant parallel seam welding packaging structure comprises the following steps:
[0013] 1) Form a cover substrate with an edge thickness of less than or equal to 0.1 mm by stamping or etching, and remove burrs;
[0014] 2) Cleaning the cover plate substrate, and then electroplating the cover plate surface to form a composite nickel plating layer to complete the corrosion resistance treatment of the cover plate;
[0015] 3) coating all areas of the processed flat-sealed shell except the sealing area with a peelable adhesive to form a plating-resistant coating;
[0016] 4) The shell body after resist plating is subjected to chemical nickel plating in a nickel plating tank as a solder layer;
[0017] 5) Remove the resist coating, clean and dry;
[0018] 6) Annealing the shell to finally form a packaging structure.
[0019] The beneficial effects of the present invention are:
[0020] 1. The chemically plated nickel layer is used as the solder layer for parallel seam welding. After the chemically plated nickel layer is melted during parallel seam welding, a high-strength connection between the tube shell and the cover plate can be achieved;
[0021] 2. The chemically plated high-phosphorus nickel layer often produces cracks due to the stress of the coating. The coating cracks on the sealing ring do not affect the role of the nickel plating layer as a solder layer;
[0022] 3. The thin cover increases the on-resistance of the cover, which makes more current pass through the sealing ring to form a loop, so that the current heat is more concentrated between the cover and the sealing ring, which promotes the melting of the electroless nickel solder layer and the combination of the molten material and the cover;
[0023] 4. The thin cover substrate is conducive to shortening the distance between the upper heating area and the lower heating area of the cover. The heat generated between the cover and the electrode is quickly transferred to the contact area between the cover and the tube shell. After the heat generated between the cover and the tube shell is superimposed, the solder layer in the sealing area is quickly melted to form a good weld.
[0024] 5. Through the optimization of structure and size, the highest heating temperature in the parallel seam welding process can be controlled to be lower than the melting point of the electroplated nickel layer. After sealing welding, there is no obvious damage to the electroplated coating on the cover plate, and the corrosion resistance of the circuit can be preliminarily judged by visual inspection;
[0025] 6. Compatible with existing parallel seam welding process;
[0026] 7. It can be processed in batches, which greatly reduces the cost of salt spray resistance of existing products. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below, but this does not limit the protection scope of the present invention.
[0028] Figure 1 It is a schematic diagram of the circuit packaging of the present invention.
[0029] Among them, 1. shell, 2. cover plate, 3. protective layer, 4. chemical nickel plating layer, 5. interconnection line, 6. chip, 7. sealing area. DETAILED DESCRIPTION
[0030] Embodiment 1:
[0031] See also Figure 1 A salt spray resistant parallel seam welding packaging structure shown includes two parts: a ceramic or metal packaging shell and an alloy cover plate; the sealing area thickness of the alloy cover plate is 0.08 to 0.1 mm; the surface of the alloy cover plate is covered with a protective layer, and the protective layer material is composite nickel plating; the protective layer is high-purity nickel formed by electroplating, and its melting point is 1455°C and the thickness is 2μm to 8.9μm; the outermost surface of the sealing area of the shell is covered with a solder layer; the solder layer is formed by chemical nickel plating, and the weight ratio of phosphorus in its nickel-phosphorus alloy is 8% to 12%, and the melting point of the nickel-phosphorus alloy is lower than 900°C.
[0032] Furthermore, the solder layer has a thickness of 2 to 5 μm.
[0033] Furthermore, the sealing area of the alloy cover plate preferably has a thickness of 0.08 mm.
[0034] Furthermore, the protective layer is high-purity nickel formed by electroplating and preferably has a thickness of 2 μm.
[0035] Furthermore, in the nickel-phosphorus alloy, the weight ratio of phosphorus is preferably 10%.
[0036] Furthermore, the melting point of the nickel-phosphorus alloy is preferably 880°C.
[0037] A method for preparing a salt spray resistant parallel seam welding packaging structure comprises the following steps:
[0038] 1) Form a cover substrate with an edge thickness of less than 0.1 mm by stamping or etching to remove burrs;
[0039] 2) Cleaning the cover plate substrate, and then electroplating the cover plate surface to form a composite nickel plating layer to complete the corrosion resistance treatment of the cover plate;
[0040] 3) coating all areas of the processed flat-sealed shell except the sealing area with a peelable adhesive to form a plating-resistant coating;
[0041] 4) The shell body after resist plating is subjected to chemical nickel plating in a nickel plating tank as a solder layer;
[0042] 5) Remove the resist coating, clean and dry;
[0043] 6) Annealing the shell to improve the bonding strength between the chemical nickel plating layer and the shell, while promoting the uniform diffusion of nickel and phosphorus in the chemical nickel plating layer to form a solder layer with a uniform melting point.
[0044] Embodiment 2: A method for preparing a salt spray resistant parallel seam welding packaging structure, comprising the following steps:
[0045] 1) forming a cover substrate with an edge thickness of 0.08 mm by stamping or etching;
[0046] 2) Cleaning the cover plate substrate, and then electroplating the cover plate surface to form a composite nickel plating layer with a thickness of 2 μm, thereby completing the corrosion resistance treatment of the cover plate;
[0047] 3) coating all areas of the processed flat-sealed shell except the sealing area with a peelable adhesive to form a plating-resistant coating;
[0048] 4) The shell body after resist plating is subjected to chemical nickel plating in a nickel plating tank as a solder layer, and the thickness of the solder layer is 2 μm;
[0049] 5) Remove the resist coating, clean and dry;
[0050] 6) Finally, the shell is annealed to improve the bonding strength between the chemical nickel plating layer and the tube shell, and at the same time promote the uniform diffusion of nickel and phosphorus in the chemical nickel plating layer to form a solder layer with a uniform melting point.
[0051] Embodiment 3: A method for preparing a salt spray resistant parallel seam welding packaging structure, comprising the following steps:
[0052] 1) forming a cover plate substrate with an edge thickness of 0.085 mm by stamping or etching;
[0053] 2) Cleaning the cover plate substrate, and then electroplating the cover plate surface to form a composite nickel plating layer with a thickness of 5 μm, thereby completing the corrosion resistance treatment of the cover plate;
[0054] 3) coating all areas of the processed flat-sealed shell except the sealing area with a peelable adhesive to form a plating-resistant coating;
[0055] 4) The shell body after resist plating is subjected to chemical nickel plating in a nickel plating tank as a solder layer, and the thickness of the solder layer is 3 μm;
[0056] 5) Remove the resist coating, clean and dry;
[0057] 6) Finally, the shell is annealed to improve the bonding strength between the chemical nickel plating layer and the tube shell, and at the same time promote the uniform diffusion of nickel and phosphorus in the chemical nickel plating layer to form a solder layer with a uniform melting point.
[0058] Embodiment 4: A method for preparing a salt spray resistant parallel seam welding packaging structure, comprising the following steps:
[0059] 1) forming a cover plate substrate with an edge thickness of 0.09 mm by stamping or etching;
[0060] 2) Cleaning the cover plate substrate, and then electroplating the cover plate surface to form a composite nickel plating layer with a thickness of 5 μm, thereby completing the corrosion resistance treatment of the cover plate;
[0061] 3) coating all areas of the processed flat-sealed shell except the sealing area with a peelable adhesive to form a plating-resistant coating;
[0062] 4) The shell body after resist plating is subjected to chemical nickel plating in a nickel plating tank as a solder layer, and the thickness of the solder layer is 4 μm;
[0063] 5) Remove the resist coating, clean and dry;
[0064] 6) Finally, the shell is annealed to improve the bonding strength between the chemical nickel plating layer and the tube shell, and at the same time promote the uniform diffusion of nickel and phosphorus in the chemical nickel plating layer to form a solder layer with a uniform melting point.
[0065] Embodiment 5: A method for preparing a salt spray resistant parallel seam welding packaging structure, comprising the following steps:
[0066] 1) forming a cover plate substrate with an edge thickness of 0.095 mm by stamping or etching;
[0067] 2) Cleaning the cover plate substrate, and then electroplating the cover plate surface to form a composite nickel plating layer with a thickness of 8 μm, thereby completing the corrosion resistance treatment of the cover plate;
[0068] 3) coating all areas of the processed flat-sealed shell except the sealing area with a peelable adhesive to form a plating-resistant coating;
[0069] 4) The shell body after resist plating is subjected to chemical nickel plating in a nickel plating tank as a solder layer, and the thickness of the solder layer is 5 μm;
[0070] 5) Remove the resist coating, clean and dry;
[0071] 6) Finally, the shell is annealed to improve the bonding strength between the chemical nickel plating layer and the tube shell, and at the same time promote the uniform diffusion of nickel and phosphorus in the chemical nickel plating layer to form a solder layer with a uniform melting point.
[0072] Embodiment 6: A method for preparing a salt spray resistant parallel seam welding packaging structure, comprising the following steps:
[0073] 1) forming a cover substrate with an edge thickness of 0.08 mm by stamping or etching;
[0074] 2) Cleaning the cover plate substrate, and then electroplating the cover plate surface to form a composite nickel plating layer with a thickness of 8 μm, thereby completing the corrosion resistance treatment of the cover plate;
[0075] 3) coating all areas of the processed flat-sealed shell except the sealing area with a peelable adhesive to form a plating-resistant coating;
[0076] 4) The shell body after resist plating is subjected to chemical nickel plating in a nickel plating tank as a solder layer, and the thickness of the solder layer is 4.5 μm;
[0077] 5) Remove the resist coating, clean and dry;
[0078] 6) Finally, the shell is annealed to improve the bonding strength between the chemical nickel plating layer and the tube shell, and at the same time promote the uniform diffusion of nickel and phosphorus in the chemical nickel plating layer to form a solder layer with a uniform melting point.
[0079] When the present invention is used, firstly, a cover plate substrate with an edge thickness of less than 0.1 mm is formed by stamping or etching; then, the cover plate substrate is cleaned, and a composite nickel plating layer with a melting point of 1455°C and a thickness of 2μm to 8.9μm is formed on the surface of the cover plate by electroplating, so as to complete the corrosion resistance treatment of the cover plate; again, a peelable adhesive is coated on all areas of the processed and formed flat-sealed shell except the sealing area to form a plating-resistant coating; the shell that has completed the plating-resistant coating is subjected to chemical nickel plating in a nickel plating tank, wherein the weight ratio of phosphorus in the nickel-phosphorus alloy is 8% to 12%, and the melting point of the nickel-phosphorus alloy is lower than 900°C, and then used as a solder layer with a thickness of 2 to 5μm; then, the plating-resistant layer is removed, and cleaning and drying are performed; finally, the shell is subjected to annealing treatment to improve the bonding strength between the chemical nickel plating layer and the tube shell, and at the same time, promote the uniform diffusion of nickel and phosphorus in the chemical nickel plating layer to form a solder layer with a uniform melting point.
[0080] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that are not conceived through creative work should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope defined in the claims.
Claims
1. A parallel seam welding packaging structure resistant to salt spray, Features: It includes two parts: a ceramic or metal packaging shell and an alloy cover plate; the base material of the alloy cover plate is Kovar or iron-nickel alloy, and the thickness of the sealing area where the alloy cover plate is located is 0.08-0.1 mm; the surface of the alloy cover plate is covered with a protective layer, which is high-purity nickel formed by electroplating, with a melting point of 1455°C and a thickness of 2μm-8.9μm; the outermost surface of the sealing area of the shell is covered with a solder layer; the solder layer is formed by chemical nickel plating, and the weight ratio of phosphorus in its nickel-phosphorus alloy is 8%-12%, and the melting point of the nickel-phosphorus alloy is lower than 900°C.
2. A salt spray resistant parallel seam welding packaging structure according to claim 1, Features: The thickness of the solder layer is 2 to 5 μm.
3. The salt spray resistant parallel seam welding packaging structure according to claim 1, Features: The sealing area of the alloy cover plate preferably has a thickness of 0.08 mm.
4. The salt spray resistant parallel seam welding packaging structure according to claim 1, Features: In the nickel-phosphorus alloy, the weight ratio of phosphorus is preferably 10%.
5. The salt spray resistant parallel seam welding packaging structure according to claim 1, Features: The melting point of the nickel-phosphorus alloy is preferably 880°C.
6. A method for preparing a salt spray resistant parallel seam welding packaging structure according to any one of claims 1 to 5, Features: The following steps are involved: 1) Form a cover substrate with an edge thickness of less than or equal to 0.1 mm by stamping or etching, and remove burrs; 2) Cleaning the cover plate substrate, and then electroplating the cover plate surface to form a composite nickel plating layer to complete the corrosion resistance treatment of the cover plate; 3) coating all areas of the processed flat-sealed shell except the sealing area with a peelable adhesive to form a plating-resistant coating; 4) The shell body after resist plating is subjected to chemical nickel plating in a nickel plating tank as a solder layer; 5) Remove the resist coating, clean and dry; 6) Annealing the shell to finally form a packaging structure.