Solid active substance battery electrode material and preparation method thereof
Through the preparation method of solid active substance battery electrode materials, the problems of uneven coating and large energy consumption in the gel-like active substance electrode materials are solved, and more uniform coating and more efficient battery production are achieved, reducing production costs and Defect rate.
Patent Information
- Application Number
- CN202411448592.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The gel-like active substances in the existing battery electrode materials have problems such as uneven coating, uneven coating density, easy defects, large energy consumption and high equipment requirements, especially the liquid slurry is prone to splash during the production process, causing defects. The drying process takes a long time and high temperature.
The preparation method of solid active substance battery electrode material, including mixing graphite, carbon black, talc powder and binder in a specific proportion, and preparing through kneading, grinding, core extrusion, sintering, oil immersion and deoiling, reducing glue and solvent dosage to improve the uniformity and production efficiency of the coating.
It effectively reduces energy consumption waste, reduces product defects, improves battery production efficiency, improves coating uniformity and surface quality, and reduces oven length and energy consumption.
Smart Images

Figure CN119008836A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery electrodes, and in particular to a solid active substance battery electrode material and a preparation method thereof. Background Art
[0002] At present, battery electrodes are mainly colloidal active substances, which are mainly mixed with active substances, solvents and colloids, and then made into a colloid, which is then transferred to the current collector for drying. The current colloidal active substances have the following disadvantages during use: ① Affected by the fluidity and shrinkage of the slurry, it is easy to cause problems such as foil leakage, wrinkles, scratches, and dark marks after coating; ② Liquid slurry is prone to splashing during the production process, resulting in dry materials adhering to the current collector and causing defects; ③ The drying process requires a longer oven and high temperature, which consumes more energy and has a large equipment volume; ④ The colloid is easy to precipitate, resulting in uneven coating surface density.
[0003] In addition, solid electrode materials are still in the research and development stage, and the main problem they face is that they cannot guarantee the stability and uniformity of the coating thickness during use.
[0004] Therefore, how to provide a solid active substance battery electrode material and a preparation method thereof to avoid the above problems is a difficult problem to be solved urgently in the art. Summary of the invention
[0005] In view of this, the present invention provides a solid active substance battery electrode material and a preparation method thereof to solve the problems of uneven slurry coating, uneven coating surface density, easy defects, high energy consumption and high equipment requirements in existing battery electrodes containing colloidal active substances.
[0006] In order to achieve the above object, the present invention adopts the following technical solution: A method for preparing a solid active substance battery electrode material comprises the following steps: After mixing the electrode components, kneading, grinding, secondary kneading, core extrusion, sintering, oil impregnation, and oil removal are sequentially performed to obtain a solid active substance battery electrode material; The electrode components include 10-80 parts of graphite, 20-80 parts of carbon black, 5-20 parts of talc, 1-10 parts of binder and 120 parts of water.
[0007] Preferably, the binder includes one or more of polyvinylidene fluoride, polyacrylic acid, carboxymethyl cellulose, UV glue and xanthan gum.
[0008] Preferably, the kneading time is 1 to 4 hours, the kneading temperature is 0° C. to 85° C., the kneading revolution speed is 20 to 300 rpm, and the kneading rotation speed is 50 to 3000 rpm.
[0009] Preferably, the grinding time is 0.5 to 3 h.
[0010] Preferably, the secondary kneading time is 0.5-2 h, the secondary kneading temperature is 0° C.-85° C., the secondary kneading revolution speed is 20-300 rpm, and the secondary kneading rotation speed is 50-3000 rpm.
[0011] Preferably, the core extrusion is performed by extruding the electrode components, and the extrusion pressure is 10-1000 kgf; The sintering temperature is 60-150°C and the sintering time is 0.5-2 h; The temperature of the immersion oil is 50-100°C and the time is 5-60 min; The deoiling time is 2 to 30 min.
[0012] Another object of the present invention is to provide a solid active substance battery electrode material prepared by the above preparation method.
[0013] It can be seen from the above technical solutions that, compared with the prior art, the present invention has the following beneficial effects: 1. The present invention reduces the amount of glue and solvent used in the preparation of traditional battery active material electrodes, effectively reduces energy consumption and waste, reduces battery manufacturing costs, and reduces product defects in the production process; 2. The present invention aims to improve the problems of leaking foil, wrinkles, scratches, dark marks, dry materials and high energy consumption that are prone to occur during the coating of battery pole pieces using liquid slurry in the prior art, especially the need to lengthen the oven and use high temperature to ensure that the coating can be dried, and the coating speed cannot be too fast. The lengthening of the oven is mainly used to increase the coating speed. The solution of the present invention can reduce the length of the oven at the same speed because the water content itself is relatively low; the solid active substance battery electrode material prepared by the present invention can be better used in battery production, improve battery production efficiency, reduce production energy consumption and improve product defects in the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0015] Figure 1 This is a physical picture of an electrode prepared using the solid active substance battery electrode material obtained in Example 1 of the present invention; Figure 2This is a physical picture of an electrode prepared using the solid active substance battery electrode material obtained in Example 2 of the present invention; Figure 3 This is a photo of an electrode prepared using the solid active substance battery electrode material obtained in Example 3 of the present invention. DETAILED DESCRIPTION
[0016] The present invention provides a method for preparing a solid active substance battery electrode material, comprising the following steps: After mixing the electrode components, kneading, grinding, secondary kneading, core extrusion, sintering, oil impregnation and oil removal are sequentially performed to obtain a solid active substance battery electrode material.
[0017] In the present invention, the electrode components include 10-80 parts of graphite, 20-80 parts of carbon black, 5-20 parts of talc, 1-10 parts of binder, and 120 parts of water; preferably, 20-40 parts of graphite, 30-50 parts of carbon black, 8-15 parts of talc, 2-8 parts of binder, and 120 parts of water; further preferably, 30 parts of graphite, 40 parts of carbon black, 10 parts of talc, 5 parts of binder, and 120 parts of water.
[0018] In the present invention, the binder includes one or more of polyvinylidene fluoride, polyacrylic acid, carboxymethyl cellulose, UV glue and xanthan gum.
[0019] In the present invention, the kneading time is 1 to 4 h, specifically 1.5 h, 2 h, 2.5 h, 3 h, and 3.5 h; the kneading temperature is 0°C to 85°C, specifically 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, and 80°C; the kneading revolution speed is 20 to 300 rpm, specifically 40 rpm, 50 rpm, 80 rpm, 100 rpm, 120 rpm, 150 rpm, 180 rpm, 200 rpm, 220 rpm, 250 rpm, and 280 rpm; the kneading rotation speed is 50 to 3000 rpm, specifically 100 rpm, 200 rpm, 500 rpm, 800 rpm, 1000 rpm, 1500 rpm, 2000 rpm, and 2500 rpm.
[0020] In the present invention, the grinding time is 0.5-3 h, specifically 1 h, 1.5 h, 2 h, 2.5 h.
[0021] In the present invention, the secondary kneading time is 0.5~2 h, specifically 0.8 h, 1 h, 1.2 h, 1.5 h, 1.6 h, 1.8 h; the secondary kneading temperature is 0°C~85°C, specifically 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C; the secondary kneading revolution speed is 20~300 rpm, specifically 40 rpm, 50 rpm, 80 rpm, 100 rpm, 120 rpm, 150 rpm, 180 rpm, 200 rpm, 220 rpm, 250 rpm, 280 rpm; the secondary kneading rotation speed is 50~3000 rpm, specifically 100 rpm, 200 rpm, 500 rpm, 800 rpm, 1000 rpm, 1500 rpm, 2000 rpm, 2500 rpm.
[0022] In the present invention, the core extrusion is performed by extrusion molding of the electrode components, and the extrusion molding pressure is 10-1000 kgf, specifically 50 kgf, 100 kgf, 200 kgf, 400 kgf, 500 kgf, 600 kgf, 800 kgf.
[0023] In the present invention, the extrusion is preferably performed using a hydraulic press.
[0024] In the present invention, the sintering temperature is 60-150°C, specifically 70°C, 80°C, 90°C, 100°C, 120°C, 140°C; the sintering time is 0.5-2 h, specifically 0.8 h, 1 h, 1.2 h, 1.4 h, 1.5 h, 1.6 h, 1.8 h.
[0025] In the present invention, the oil immersion temperature is 50-100°C, specifically 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C; the oil immersion time is 5-60 min, specifically 10 min, 20 min, 30 min, 40 min, 50 min.
[0026] In the present invention, the oil immersion is preferably carried out in an oil immersion pan, preferably with silicone oil, the role of the oil immersion is to make it smooth and lubricated, soft, and not easy to break.
[0027] In the present invention, the deoiling time is 2 to 30 min, specifically 5 min, 10 min, 15 min, 20 min, or 15 min.
[0028] In the present invention, the deoiling is preferably carried out using a centrifugal deoiler.
[0029] The present invention also provides a solid active substance battery electrode material prepared by the above preparation method.
[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] Battery electrode components: The weight proportions of the components are: 50 parts of graphite, 35 parts of carbon black, 10 parts of talc, 5 parts of polyvinylidene fluoride (PVDF), and 120 parts of water.
[0033] Preparation process: The components are mixed according to the weight portions, kneaded in a kneader at 20°C for 3 h, the revolution speed of the kneading is 100 rpm, the rotation speed is 500 rpm, and after the kneading is completed, it is ground in a three-roll grinder for 1 h, and then kneaded for a second time in a secondary kneader at 20°C for 1 h, the revolution speed of the second kneading is 100 rpm, and the rotation speed is 500 rpm. After the core is extruded at 800 kgf in a hydraulic press, it is dried in a core drying furnace, sintered at 100°C in an electric tunnel kiln for 1 h, immersed in oil at 80°C in an oil immersion pot (methyl silicone oil) for 30 min, and deoiled in a centrifugal deoiler for 10 min to obtain a solid active substance battery electrode material, and then the block product is rubbed and coated on a coating machine, and then baked in an oven to obtain a battery electrode sheet, such as Figure 1 .pass Figure 1 It can be seen that the surface quality of the product after rubbing and coating is fine, without problems such as foil leakage, scratches, dark marks, etc. The color is soft and delicate, with a color of 55 (representing the consistency of the surface density of the electrode and the uniformity of the coating).
[0034] Example 2 Battery electrode components: The weight proportions of the components are: 40 parts of graphite, 45 parts of carbon black, 10 parts of talc, 5 parts of polyacrylic acid (PAA), and 120 parts of water.
[0035] The preparation process is the same as in Example 1, and the obtained battery electrode sheet is as follows Figure 2 As shown. Figure 2 It can be seen that the surface quality of the product after rubbing and coating is fine, without problems such as foil leakage, scratches, dark marks, etc. The color is soft and delicate, with a color of 41 (representing the consistency of the surface density of the electrode and the uniformity of the coating).
[0036] Example 3
[0037] Battery electrode components: The weight proportions of the components are: 30 parts of graphite, 55 parts of carbon black, 10 parts of talc, 5 parts of carboxymethyl cellulose (CMC), and 120 parts of water.
[0038] The preparation process is the same as in Example 1, and the obtained battery electrode sheet is as follows Figure 3 As shown. Figure 3 It can be seen that the surface quality of the product after rubbing and coating is fine, without problems such as foil leakage, scratches, dark marks, etc. The color is soft and delicate, with a color of 36 (representing the consistency of the surface density of the electrode and the uniformity of the coating).
[0039] Example 4
[0040] Battery electrode components: The weight proportions of the components are: 80 parts of graphite, 60 parts of carbon black, 5 parts of talc, 10 parts of polyvinylidene fluoride (PVDF), and 120 parts of water.
[0041] Preparation process: The components are mixed according to the weight portions, kneaded in a kneader at 50°C for 1 h, the revolution speed of the kneading is 200 rpm, the rotation speed is 1000 rpm, and after kneading, they are ground in a three-roll grinder for 2 h, and then kneaded for a second time at 20°C in a secondary kneader for 0.5 h, the revolution speed of the second kneading is 200 rpm, and the rotation speed is 800 rpm. After the core is extruded at 200 kgf in a hydraulic press, it is dried in a core drying furnace, sintered at 60°C in an electric tunnel kiln for 2 h, immersed in oil at 100°C in an oil immersion pot (methyl silicone oil) for 20 min, and deoiled in a centrifugal deoiler for 15 min to obtain a solid active substance battery electrode material.
[0042] Example 5 Battery electrode components: The weight proportions of the components are: 20 parts of graphite, 20 parts of carbon black, 6 parts of talc, 3 parts of carboxymethyl cellulose (CMC), and 120 parts of water.
[0043] Preparation process: The components are mixed according to the weight portions, kneaded in a kneader at 10°C for 4 h, the revolution speed of the kneading is 50 rpm, the rotation speed is 200 rpm, and after kneading, it is ground in a three-roll grinder for 3 h, and then kneaded for a second time in a secondary kneader at 20°C for 1.5 h, the revolution speed of the second kneading is 50 rpm, and the rotation speed is 200 rpm. After the core is extruded at 500 kgf in a hydraulic press, it is dried in a core drying furnace, sintered at 150°C in an electric tunnel kiln for 2 h, immersed in oil at 50°C in an oil immersion pot (methyl silicone oil) for 50 min, and deoiled in a centrifugal deoiler for 30 min to obtain a solid active substance battery electrode material.
[0044] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0045] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a solid active substance battery electrode material, characterized in that: The steps include: After mixing the electrode components, kneading, grinding, secondary kneading, core extrusion, sintering, oil impregnation, and oil removal are sequentially performed to obtain a solid active substance battery electrode material; The electrode components include 10-80 parts of graphite, 20-80 parts of carbon black, 5-20 parts of talc, 1-10 parts of binder and 120 parts of water.
2. The method for preparing a solid active substance battery electrode material according to claim 1, characterized in that: The binder includes one or more of polyvinylidene fluoride, polyacrylic acid, carboxymethyl cellulose, UV glue and xanthan gum.
3. The method for preparing a solid active substance battery electrode material according to claim 2, characterized in that: The kneading time is 1-4 h, the kneading temperature is 0-85° C., the kneading revolution speed is 20-300 rpm, and the kneading rotation speed is 50-3000 rpm.
4. The method for preparing a solid active substance battery electrode material according to any one of claims 1 to 3, characterized in that: The grinding time is 0.5 to 3 h.
5. The method for preparing a solid active substance battery electrode material according to claim 4, characterized in that: The secondary kneading time is 0.5-2 h, the secondary kneading temperature is 0-85° C., the secondary kneading revolution speed is 20-300 rpm, and the secondary kneading rotation speed is 50-3000 rpm.
6. The method for preparing a solid active substance battery electrode material according to claim 5, characterized in that: The core extrusion is to extrude the electrode components, and the extrusion pressure is 10-1000 kgf; The sintering temperature is 60-150°C and the sintering time is 0.5-2 h; The temperature of the immersion oil is 50-100°C and the time is 5-60 min; The deoiling time is 2 to 30 min.
7. A solid active substance battery electrode material prepared by the method for preparing a solid active substance battery electrode material according to any one of claims 1 to 6.
Citation Information
Patent Citations
Oleophylic sulfur electrode preparation method
CN104716297A
Matte pencil lead and preparation method thereof
CN109385147A
Battery electrode plate viscoelastic raw material, raw material preparation method and electrode plate preparation method
CN109616635A
Lithium ion battery electrode paste semidry method dispensing process, lithium ion battery positive electrode sheet, lithium ion battery negative electrode sheet, and lithium ion battery
CN110600671A
Lithium ion battery negative electrode slurry and preparation process thereof
CN116826055A