Porous silicon carbon negative electrode, solid-state battery and preparation method
By using porous silicon carbon negative electrodes and specific binders in solid-state batteries, the silicon-based negative electrode volume expansion and cycle stability problems are solved, and higher cycle stability and lithium ion transmission performance are achieved, improving the overall performance of solid-state batteries. .
Patent Information
- Application Number
- CN202410920865.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The silicon-based negative electrode in solid-state batteries has problems of volume expansion and poor cycle stability, resulting in structural failure and low cycling Coulomb efficiency.
Using porous silicon carbon anode, including porous silicon carbon, conductive carbon black and specific binders (such as polyvinylidene fluoride, polyacrylic acid, polyacrylonitrile and carboxymethylcellulose), through rich pore structure and high mechanical strength The adhesive buffers volume expansion and maintains electrode structural integrity.
It improves the cycle stability and lithium ion transmission performance of solid-state batteries, avoids the breaking of silicon particles, and enhances the mechanical stability and capacity storage rate of the battery.
Smart Images

Figure CN119008858A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid-state batteries, and in particular to a porous silicon-carbon negative electrode, a solid-state battery and a preparation method thereof. Background Art
[0002] As the environmental situation becomes increasingly severe, the efficient development and utilization of new energy has become a contemporary theme. At present, commercial liquid lithium-ion batteries have been widely used in electric vehicles, mobile phones, laptops, and large-scale energy storage. In recent years, the fields of electric vehicles and energy storage have developed rapidly, but accidents such as battery spontaneous combustion and fires in energy storage stations have occurred frequently, and people have put forward higher requirements for the safety of lithium-ion batteries. Liquid batteries use flammable organic liquids as electrolytes. After a short circuit occurs, thermal runaway occurs, the battery will burn violently or even cause an explosion, causing serious safety problems and becoming an obstacle to the large-scale application of batteries. The use of non-flammable solid electrolytes in solid-state batteries can effectively prevent the safety problems caused by the use of flammable organic electrolytes in liquid batteries.
[0003] Silicon is the second most abundant element on earth. Silicon-based anode is an anode material with extremely high theoretical specific capacity (3579mAh / g), and it has a suitable lithium insertion potential, with an operating potential of about 0.4V, which can effectively avoid the problem of lithium dendrite growth. It has attracted widespread attention from researchers in recent years. It is an effective alternative before the full commercialization of lithium metal anodes, and it is also one of the key research contents of solid-state batteries. However, the pure silicon anode in solid-state batteries will produce a dramatic volume expansion during the lithiation process, resulting in silicon particle breakage and electrode structure failure; in addition, silicon, as an intrinsic semiconductor, has low electronic conductivity, which makes the pure silicon anode have poor cycle stability and low cycle coulomb efficiency. The refinement of silicon particles to nanometer level can avoid the problem of particle breakage during the first charge and discharge process, thereby improving the cycle stability to a certain extent, but it still cannot meet the needs of practical applications. Therefore, it is urgent to develop a silicon-based anode formula suitable for solid-state batteries to inhibit volume expansion and improve cycle stability.
[0004] The silicon-based negative electrode in the solid-state battery is mainly composed of three parts: active material, conductive agent and binder. Among them, the active material is the main material that exerts performance, but the conductive agent and binder are also crucial to improving the stability and dynamics of the electrode. In liquid batteries, the binder system of silicon-based negative electrodes has been widely studied. By designing the functional groups and structures of the binders, the core indicators of the silicon-based negative electrode, such as tensile strength, elongation at break, self-healing ability, and ion / electron conduction, can be improved, thereby improving the cycle stability and rate performance of the silicon-based negative electrode, which is one of the current mainstream research contents. However, in the solid-state battery system, the silicon-based negative electrode cannot achieve the wetting effect in the liquid battery. It is usually necessary to apply a large external pressure to ensure the solid-solid contact between the silicon-based negative electrode and the electrolyte, and the environment of the binder is very different from that in the liquid system. Therefore, it is crucial to screen a suitable binder system and optimize the interface design for the operating environment of the silicon-based negative electrode in the solid-state battery for the stable operation of the solid-state battery.
[0005] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0006] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a porous silicon-carbon negative electrode, a solid-state battery and a preparation method, aiming to solve the problems of volume expansion and poor cycle stability of silicon-based negative electrodes in existing solid-state batteries.
[0007] The technical solution of the present invention is as follows:
[0008] According to a first aspect of the present invention, a porous silicon-carbon negative electrode is provided, comprising a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector, wherein the negative electrode active material layer comprises porous silicon carbon, conductive carbon black and a binder, and the binder comprises at least one of polyvinylidene fluoride, polyacrylic acid, polyacrylonitrile and carboxymethyl cellulose.
[0009] Optionally, the binder is polyvinylidene fluoride.
[0010] Optionally, the porous silicon carbon is powdered porous silicon carbon, the particle size of the powdered porous silicon carbon is 1-30 μm, wherein the particle size of nano silicon is 50-200 nm.
[0011] Optionally, the mass ratio of the porous silicon carbon, the conductive carbon black and the binder is 80-95:5:1-15.
[0012] The second aspect of the present invention provides a method for preparing the porous silicon-carbon negative electrode according to the present invention, which comprises the steps of:
[0013] Dispersing a binder in a solvent and stirring to obtain a binder solution;
[0014] The porous silicon carbon, the conductive carbon black and the binder solution are mixed and stirred to obtain a negative electrode slurry;
[0015] The negative electrode slurry is coated on a negative electrode current collector, and the solvent is removed to obtain the porous silicon-carbon negative electrode.
[0016] Optionally, the coating thickness of the negative electrode slurry is 40-110 μm.
[0017] A third aspect of the present invention provides a solid-state battery, comprising a solid electrolyte layer and the porous silicon-carbon negative electrode of the present invention bonded to one side of the solid electrolyte layer.
[0018] Optionally, the solid electrolyte layer includes a sulfide solid electrolyte.
[0019] A fourth aspect of the present invention provides a method for preparing a solid-state battery, comprising the steps of:
[0020] providing a solid electrolyte layer;
[0021] The porous silicon-carbon negative electrode of the present invention is attached to one side of the solid electrolyte layer, and cold pressed to tightly combine the porous silicon-carbon negative electrode and the solid electrolyte layer;
[0022] The positive electrode is attached to the other side of the solid electrolyte layer, and cold pressing is performed to make the positive electrode and the solid electrolyte layer in close contact, thereby obtaining the solid-state battery.
[0023] Optionally, the cold pressing pressure is 250-450 MPa.
[0024] Beneficial effects: For the solid-state battery system, a porous silicon-carbon negative electrode is used. The rich pore structure inside the porous carbon can well accommodate and buffer the volume expansion of the silicon material, ensuring the ion transmission during the cycle process. It has excellent lithium ion transmission performance and good mechanical stability. It can prevent silicon particles from being squeezed and crushed due to mutual squeezing during volume expansion, and buffer the capacity attenuation of the silicon-based negative electrode under the premise of high energy density; the matching binder has high mechanical strength and elongation at break, and can still maintain the integrity of the porous silicon-carbon negative electrode structure under the combined stress of large external pressure and silicon volume expansion, thereby improving the cycle stability of the solid-state battery; the added conductive carbon black ensures the electrical contact of the porous silicon-carbon material after volume expansion, which greatly improves the cycle stability of the solid-state battery, and the first efficiency and capacity retention rate are good. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A comparison chart of the cycle curves of the solid-state batteries prepared in Examples 1-7 and Comparative Examples 1-2 provided by the present invention.
[0026] Figure 2This is a SEM image of the electrode of Example 1 provided by the present invention after 10 cycles. DETAILED DESCRIPTION
[0027] The present invention provides a porous silicon-carbon negative electrode, a solid-state battery and a preparation method. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0028] The current solid-state battery's sheet-like silicon-based negative electrode has not solved the problem of poor silicon conductivity, and the silicon lacks internal buffering when it repeatedly expands in volume, which can easily lead to the destruction of the integrity of the silicon-based negative electrode structure, thereby causing a decrease in the cycle stability of the silicon-based negative electrode; and the solid-state battery requires high pressure operation, which severely limits its practical application; in addition, the binder in the solid-state battery is subjected to the combined stress of external pressure and silicon volume expansion, and without the infiltration of electrolyte, the plasticization effect cannot be achieved.
[0029] Based on this, an embodiment of the present invention provides a porous silicon-carbon negative electrode, wherein the porous silicon-carbon negative electrode includes porous silicon carbon, conductive carbon black and a binder; the binder includes at least one of polyvinylidene fluoride (PVDF), polyacrylic acid (PAA), polyacrylonitrile (PAN) and carboxymethyl cellulose (CMC).
[0030] In an embodiment of the present invention, a porous silicon-carbon negative electrode is used for a solid-state battery system. The rich pore structure inside the porous carbon can well accommodate and buffer the volume expansion of the silicon material, ensure ion transmission during the cycle process, have excellent lithium ion transmission performance, and have good mechanical stability. It can prevent silicon particles from being squeezed and crushed due to mutual expansion, and buffer the capacity decay of the silicon-based negative electrode under the premise of high energy density; the matching binder has high mechanical strength and elongation at break, and can still maintain the integrity of the porous silicon-carbon negative electrode structure under the combined stress of large external pressure and silicon volume expansion, thereby improving the cycle stability of the solid-state battery; the added conductive carbon black ensures the electrical contact of the porous silicon-carbon material after volume expansion, so that the cycle stability of the solid-state battery is greatly improved, and the first efficiency and capacity retention rate are good.
[0031] Preferably, the binder is PVDF.
[0032] In view of the external pressure of the solid-state battery system and the cycle, a more suitable binder PVDF was selected, which is different from the PAA binder commonly used in silicon-based negative electrode liquid batteries. This is because under large external pressure, PVDF binder has higher mechanical strength and elongation at break than PAA, CMC, and PAN binders commonly used in liquid batteries, and has excellent bonding properties in the absence of electrolyte infiltration. It can still maintain structural integrity under the combined stress of large external pressure and silicon volume expansion, thereby improving the cycle stability of solid-state batteries.
[0033] In an embodiment of the present invention, the porous silicon carbon is a vapor-deposited porous silicon carbon, which is a material in which nano-silicon particles are deposited inside a porous carbon skeleton, and then the silicon carbon skeleton is coated with carbon. The porous silicon carbon can be purchased commercially, for example, from Shenzhen Solid New Material Technology Co., Ltd.
[0034] In one embodiment, the porous silicon carbon is powdered porous silicon carbon, the particle size of the powdered porous silicon carbon is 1-30 μm, wherein the particle size of nano silicon is 50-200 nm.
[0035] The mass percentage of nano-silicon in the porous silicon carbon is 40%-60%. The porous carbon in this ratio range can well accommodate the volume expansion of silicon particles and ensure the high specific capacity of silicon-based negative electrode materials. The high specific capacity of the porous silicon carbon can be as high as 1600-2300mAh / g.
[0036] In one embodiment, the mass ratio of the porous silicon carbon, the conductive carbon black and the binder is 80-95:5:1-15.
[0037] Preferably, the mass ratio of the porous silicon carbon, the conductive carbon black and the binder is 90:5:5.
[0038] An embodiment of the present invention provides a method for preparing the porous silicon-carbon negative electrode as described above, which comprises the steps of:
[0039] (1) dispersing a binder in a solvent and stirring to obtain a binder solution;
[0040] (2) mixing porous silicon carbon, conductive carbon black and a binder solution, and stirring to obtain a negative electrode slurry;
[0041] (3) The negative electrode slurry is coated on a negative electrode current collector, and after removing the solvent, the porous silicon-carbon negative electrode is obtained.
[0042] In one embodiment, step (1) specifically includes: dispersing the binder in a solvent, and stirring at room temperature to obtain a uniformly dispersed binder solution.
[0043] In one embodiment, the negative electrode current collector is copper foil, because copper foil has high conductivity, good ductility, and is stable at low potential.
[0044] In one embodiment, the solvent may be selected from at least one of N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), and water.
[0045] In one embodiment, step (2) specifically includes: mixing porous silicon carbon, conductive carbon black and a binder solution in a certain proportion, and stirring at room temperature to obtain a uniform negative electrode slurry.
[0046] In one embodiment, step (3) specifically includes: coating the negative electrode slurry on a copper foil, drying it in a forced air oven to remove most of the solvent, and then drying it in a vacuum oven to completely remove the solvent to obtain the porous silicon-carbon negative electrode.
[0047] Wherein, the drying temperature may be 70-100°C.
[0048] In one embodiment, the coating thickness of the negative electrode slurry is 40-110 μm, such as 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, etc. This moderate thickness can ensure lithium ion conduction inside the battery while providing high capacity, further ensuring stable operation of the battery.
[0049] An embodiment of the present invention provides a solid-state battery, which includes a solid electrolyte layer and the porous silicon-carbon negative electrode combined with one side of the solid electrolyte layer.
[0050] In an embodiment of the present invention, a porous silicon-carbon negative electrode is used for a solid-state battery system. The porous silicon-carbon negative electrode has excellent lithium ion transmission performance and excellent electrical conductivity. At the same time, the rich pore structure inside the porous carbon can accommodate and buffer the volume expansion of silicon to a certain extent, ensuring ion transmission during the cycle process, and has good mechanical stability, which can prevent silicon particles from being crushed due to mutual squeezing during volume expansion, and buffer the capacity decay of the porous silicon-carbon negative electrode under the premise of high energy density. In order to ensure the cycle stability of the solid-state battery, a certain amount of conductive carbon black is added to ensure electrical contact of the porous silicon-carbon material after volume expansion.
[0051] In one embodiment, the solid electrolyte layer includes a sulfide solid electrolyte. As an example, the sulfide solid electrolyte may be Li 6 PS 5 Cl, Li 3 PS 4 , Li 4 S N 4 , Li 7 P3 S 11 At least one of the following, but not limited to.
[0052] In one embodiment, the sulfide solid electrolyte is a granular sulfide solid electrolyte, and the particle size of the granular sulfide solid electrolyte is 1-20 μm.
[0053] An embodiment of the present invention provides a method for preparing a solid-state battery, which comprises the following steps:
[0054] providing a solid electrolyte layer;
[0055] The porous silicon-carbon negative electrode is attached to one side of the solid electrolyte layer, and cold pressed to tightly combine the porous silicon-carbon negative electrode and the solid electrolyte layer;
[0056] The positive electrode is attached to the other side of the solid electrolyte layer, and cold pressing is performed to make the positive electrode and the solid electrolyte layer in close contact, thereby obtaining the solid-state battery.
[0057] In one embodiment, the solid electrolyte layer can be prepared by the following method: weigh a certain amount of solid electrolyte, put it into a solid-state battery mold, and cold press it to obtain the solid electrolyte layer.
[0058] In one embodiment, in the step of cold pressing to tightly bond the porous silicon-carbon negative electrode and the solid electrolyte layer, the pressure of the cold pressing is 250-450 MPa.
[0059] In one embodiment, the step of attaching the positive electrode to the other side of the solid electrolyte layer and cold pressing the positive electrode to make close contact with the solid electrolyte layer to obtain the solid-state battery specifically includes: attaching a lithium sheet and an indium sheet to the other side of the solid electrolyte layer in sequence, then placing a copper current collector, and cold pressing the lithium and indium to make them tightly combined and in close contact with the solid electrolyte layer to obtain the solid-state battery.
[0060] In one embodiment, the ratio of the mass of lithium to the sum of the mass of lithium and indium in step (3) is between 30% and 55%.
[0061] In one embodiment, in the step of cold pressing to tightly combine lithium and indium and to tightly contact the solid electrolyte layer, the pressure of the cold pressing is 250-450 MPa.
[0062] After solid-state batteries are assembled, they operate under a certain external pressure.
[0063] In one embodiment, the external pressure is 20-70 MPa, such as 20 MPa, 30 MPa, 40 MPa, 50 MPa, 60 MPa, 70 MPa, etc.
[0064] Preferably, the external pressure is 60 MPa. When operated under this external pressure, the solid-state battery has more excellent cycle stability, good first efficiency and capacity retention rate.
[0065] The present invention will be further described below by means of specific examples.
[0066] Example 1
[0067] The PVDF binder is dissolved in N-methylpyrrolidone (NMP) solvent to prepare a binder solution with a mass concentration of 3%; a porous silicon-carbon powder with a particle size of 5-10 μm is selected as the active material, and a slurry is prepared according to a mass ratio of the active material, conductive carbon black and the binder of 90:5:5, and the mixture is stirred and mixed at room temperature. A scraper is used to scrape the mixed slurry on a copper foil, and the thickness of the slurry coated on the copper foil is 50 μm. After drying in a blast oven to remove most of the solvent, vacuum drying is performed to completely remove the solvent to obtain a porous silicon-carbon negative electrode.
[0068] Weigh 150 mg of solid electrolyte Li 6 PS 5 Cl, put it into a solid-state battery mold, and obtain a solid electrolyte layer by cold pressing. The porous silicon-carbon negative electrode is attached to one side of the solid electrolyte layer, and the porous silicon-carbon negative electrode and the solid electrolyte layer are tightly combined by cold pressing at a pressure of 350Mpa. The lithium sheet and the indium sheet are attached to the other side of the solid electrolyte layer in sequence, and then the copper current collector is placed, and the lithium and indium are tightly combined and in close contact with the solid electrolyte layer by cold pressing.
[0069] After the solid-state battery is assembled, it operates under an external pressure of 60Mpa.
[0070] Example 2
[0071] The PAA binder was dissolved in N-methylpyrrolidone (NMP) solvent to prepare a binder solution with a mass concentration of 3%; the rest was the same as in Example 1.
[0072] Example 3
[0073] The mass ratio of active material, conductive carbon black and binder is 95:0:5; the rest is the same as Example 1.
[0074] Example 4
[0075] The PAA binder was dissolved in N-methylpyrrolidone (NMP) solvent to prepare a binder solution with a mass concentration of 3%; the mass ratio of the active material, the conductive carbon black and the binder was 95:0:5; the rest was the same as Example 1.
[0076] Example 5
[0077] The CMC binder was dissolved in water to prepare a binder solution with a mass concentration of 3%; the rest was the same as in Example 1.
[0078] Example 6
[0079] The PAN binder was dissolved in N,N-dimethylformamide (DMF) solvent to prepare a binder solution with a mass concentration of 3%; the rest was the same as in Example 1.
[0080] Example 7
[0081] After the battery is assembled, it is operated under an external pressure of 50 MPa; the rest is the same as in Example 1.
[0082] Comparative Example 1
[0083] Nano silicon powder with a particle size of 80-120 nm was selected as the active material; the rest was the same as in Example 1.
[0084] Comparative Example 2
[0085] Nano silicon carbon powder with a particle size of 80-120 nm was selected as the active material; the rest was the same as in Example 1.
[0086] The electrochemical performance test method is as follows: the assembled battery is subjected to long electrochemical cycles, the voltage range is set to -0.595V-0.88V, after activating for one cycle at a rate of 0.1C, a long cycle test is performed at a rate of 0.33C. The test results are shown in Table 1 and Figure 1 .
[0087] Table 1. Electrochemical performance test results of each battery
[0088]
[0089]
[0090] Depend on Figure 1 As shown in Table 1, for the solid-state battery system, the use of porous silicon-carbon negative electrode and the selection of suitable binders and the addition of conductive agents can ensure the conduction of electrons and ions inside the electrode, reduce impedance, and improve the cycle stability of the battery. The capacity retention rate after 150 cycles can reach 78.89%, which is much higher than nano-silicon (31.75%) and nano-silicon carbon (24.73%).
[0091] Figure 2 This is a SEM image of the porous silicon-carbon negative electrode of the battery in Example 1 after 10 cycles. After 10 cycles, silicon undergoes an amorphous transformation during lithium insertion, the elastic modulus is significantly reduced, and plastic deformation occurs, forming a relatively dense block, which can ensure effective electron and ion conduction between particles.
[0092] In summary, the present invention provides a porous silicon-carbon negative electrode, a solid-state battery and a preparation method. The porous silicon-carbon negative electrode is used for the solid-state battery system. The rich pore structure inside the porous carbon can well accommodate and buffer the volume expansion of the silicon material, ensure the ion transmission during the cycle process, have excellent lithium ion transmission performance, and have good mechanical stability, which can prevent the silicon particles from being squeezed and crushed due to mutual squeezing during volume expansion, and buffer the capacity attenuation of the silicon-based negative electrode under the premise of high energy density; the matching binder has high mechanical strength and elongation at break, and can still maintain the integrity of the porous silicon-carbon negative electrode structure under the combined stress of large external pressure and silicon volume expansion, thereby improving the cycle stability of the solid-state battery; the added conductive carbon black ensures the electrical contact of the porous silicon-carbon material after volume expansion, so that the cycle stability of the solid-state battery is greatly improved, and the first efficiency and capacity retention rate are good.
[0093] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A porous silicon-carbon negative electrode, comprising a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector, characterized in that: The negative electrode active material layer includes porous silicon carbon, conductive carbon black and a binder, wherein the binder includes at least one of polyvinylidene fluoride, polyacrylic acid, polyacrylonitrile and carboxymethyl cellulose.
2. The porous silicon-carbon negative electrode according to claim 1, characterized in that: The binder is polyvinylidene fluoride.
3. The porous silicon-carbon negative electrode according to claim 1, characterized in that: The porous silicon carbon is powdered porous silicon carbon, the particle size of the powdered porous silicon carbon is 1-30 μm, wherein the particle size of nano silicon is 50-200 nm.
4. The porous silicon-carbon negative electrode according to claim 1, characterized in that: The mass ratio of the porous silicon carbon, the conductive carbon black and the binder is 80-95:5:1-15.
5. A method for preparing a porous silicon-carbon negative electrode according to any one of claims 1 to 4, characterized in that: Includes steps: Dispersing a binder in a solvent and stirring to obtain a binder solution; The porous silicon carbon, the conductive carbon black and the binder solution are mixed and stirred to obtain a negative electrode slurry; The negative electrode slurry is coated on a negative electrode current collector, and the solvent is removed to obtain the porous silicon-carbon negative electrode.
6. The method for preparing a porous silicon-carbon negative electrode according to claim 5, characterized in that: The coating thickness of the negative electrode slurry is 40-110 μm.
7. A solid-state battery, characterized in that: A porous silicon-carbon negative electrode according to any one of claims 1 to 4, comprising a solid electrolyte layer and the porous silicon-carbon negative electrode combined with one side of the solid electrolyte layer.
8. The solid-state battery according to claim 7, characterized in that: The solid electrolyte layer includes a sulfide solid electrolyte.
9. A method for preparing a solid-state battery, characterized in that: Includes steps: providing a solid electrolyte layer; Attaching the porous silicon-carbon negative electrode according to any one of claims 1 to 4 to one side of the solid electrolyte layer, and cold pressing to tightly combine the porous silicon-carbon negative electrode and the solid electrolyte layer; The positive electrode is attached to the other side of the solid electrolyte layer, and cold pressing is performed to make the positive electrode and the solid electrolyte layer in close contact, thereby obtaining the solid-state battery.
10. The method for preparing a solid-state battery according to claim 9, characterized in that: The cold pressing pressure is 250-450Mpa.
Citation Information
Patent Citations
Negative electrode of solid-state lithium electrode and preparation method and application thereof
CN108288690A
Negative electrode material, negative electrode plate and battery
CN116053447A
Solid-state battery and preparation method thereof
CN116525966A
Cited By
Flexible solid-state lithium ion battery and preparation method thereof
CN119601748A
Silicon-based solid-state battery and preparation method thereof
CN119764579A
Silicon-based solid-state battery and preparation method thereof
CN119764579B
Silicon-carbon negative electrode material applied to sulfide solid-state battery and modification method of silicon-carbon negative electrode material
CN120237195A
Silicon-carbon anode materials for use in sulfide solid-state batteries and their modification methods
CN120237195B