High-compaction rate type long-circulation lithium iron phosphate positive electrode material as well as preparation method and application of high-compaction rate type long-circulation lithium iron phosphate positive electrode material

By using resin-based asphalt with a β resin content of 45%-55% as the carbon source, hard carbon and soft carbon structures are formed to coat lithium iron phosphate materials, the problem of reducing compaction performance caused by carbon coating in the prior art is solved. Significantly improves the circulation and rate performance of the material.

CN119008914APending Publication Date: 2024-11-22JIANGXI ANCHI NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411352611.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the existing modification methods, the use of glucose, sucrose, white sugar or PEG for carbon coating has led to a decrease in the compaction and electrochemical properties of the lithium iron phosphate positive electrode material.

Method used

Resin-based asphalt with a β resin content of 45%-55% is used as the carbon source, and hard carbon and soft carbon structures are formed through sintering, uniformly coated on the surface of lithium iron phosphate material to form a stable core-shell structure, and improve compaction density and circulation. performance.

Benefits of technology

The cycling and rate-efficiency performance of lithium iron phosphate positive electrode material is improved, and the cladding layer formed is uniform and dense, which significantly improves the electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005062751930000051
    Figure BDA0005062751930000051
Patent Text Reader

Abstract

The invention provides a high-compaction rate type long-circulation lithium iron phosphate positive electrode material as well as a preparation method and application thereof. The method comprises the following steps: mixing iron phosphate and lithium carbonate with water, and sanding to obtain slurry; adding resin-based asphalt into an ethanol solvent, heating, stirring and dissolving to obtain an asphalt solution; adding the slurry into an asphalt solution, and sanding to obtain a mixed solution; carrying out spray drying on the mixed solution to obtain a positive electrode material precursor; and sintering the positive electrode material precursor at a high temperature under the protection of an inert atmosphere, cooling to room temperature, and crushing to obtain the positive electrode material. The resin-based asphalt with the beta resin content of 45%-55% is used as a carbon source, and the beta resin has good bonding strength, forms hard carbon and soft carbon structures in the sintering process, and can uniformly coat the outer surface of the lithium iron phosphate material to form a stable core-shell structure, so that the prepared positive electrode material is high in compaction density, a formed coating layer is uniform and compact, and the service life of the positive electrode material is prolonged. And the cycle performance and the rate capability are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a high-density long-cycle lithium iron phosphate positive electrode material and a preparation method and application thereof. Background Art

[0002] Lithium batteries are a type of battery that uses lithium metal or lithium alloy as positive / negative electrode materials and non-aqueous electrolyte solutions. In 1912, lithium metal batteries were first proposed and studied by Gilbert N. Lewis. In the 1970s, MS Whittingham proposed and began to study lithium-ion batteries. Due to the very active chemical properties of lithium metal, the processing, storage, and use of lithium metal have very high environmental requirements. With the development of science and technology, lithium batteries have become mainstream.

[0003] Lithium iron phosphate has attracted widespread attention since it was proposed in 1997. It occupies a place in lithium-ion battery positive electrode materials with its excellent stability, high-rate charging, non-toxicity and long cycle life. However, as a positive electrode material, lithium iron phosphate also has obvious defects such as low electrical conductivity and ion diffusion rate.

[0004] As far as positive electrode materials are concerned, low conductivity greatly limits the performance of lithium iron phosphate batteries. In order to improve the conductivity of lithium iron phosphate, current improvement methods include carbon coating, metal doping, adding metal particles, etc., which can increase the conductivity by several orders of magnitude. In the production process of LFP, carbon sources are often used as reducing agents. The addition of carbon sources can form a carbon coating on the surface of lithium iron phosphate to enhance the conductivity of the particles. Usually, carbon coating uses glucose, sucrose, white sugar or PEG, etc., but these carbon source coatings will also cause the compaction performance of the positive electrode material to decrease, thereby reducing the electrochemical performance. Summary of the invention

[0005] The present invention provides a high compaction rate long cycle lithium iron phosphate positive electrode material and a preparation method and application thereof, the purpose of which is to solve the problems of reduced compaction performance and reduced electrochemical performance of the positive electrode material caused by the existing modification method using glucose, sucrose, white sugar or PEG for carbon coating.

[0006] In order to achieve the above-mentioned purpose, an embodiment of the present invention provides a high compaction rate type long cycle lithium iron phosphate positive electrode material and its preparation method and application. The present invention adopts resin-based asphalt with a β resin content of 45%-55% as the carbon source. Since the β resin has a high bonding strength, a hard carbon plus soft carbon structure is formed during the sintering process, which can be evenly coated on the outer surface of the lithium iron phosphate material to form a stable core-shell structure with high compaction density. The formed coating layer is uniform and dense, and both the cycle performance and the rate performance are improved.

[0007] An object of an embodiment of the present invention is to provide a method for preparing a high-density long-cycle lithium iron phosphate positive electrode material, comprising the following steps:

[0008] S1: iron phosphate and lithium carbonate are mixed with water and sand-milled to obtain slurry;

[0009] S2: taking resin-based asphalt and adding it to ethanol solvent, heating and stirring to dissolve, to obtain an asphalt solution;

[0010] S3: adding the slurry to the asphalt solution and performing sand milling to obtain a mixed solution;

[0011] S4: spray drying the mixed solution to obtain a positive electrode material precursor;

[0012] S5: Sintering the cathode material precursor at high temperature under the protection of an inert atmosphere, and then crushing it after cooling to room temperature to obtain the cathode material precursor.

[0013] According to one aspect of the embodiment of the present invention, in step S1, the particle size D50 after sand grinding is 0.8-1.2 μm.

[0014] According to one aspect of the embodiment of the present invention, in step S2, the heating temperature is 45-80°C and the time is 2-8h.

[0015] According to one aspect of the embodiment of the present invention, in step S2, the β resin content of the resin-based asphalt is 45% to 55%.

[0016] According to one aspect of the embodiment of the present invention, in step S3, the particle size D50 after sand grinding is 0.6-1.0 μm.

[0017] According to one aspect of the embodiment of the present invention, in step S4, the spray drying temperature is 90-250° C. and the time is 4-5 hours.

[0018] According to one aspect of the embodiment of the present invention, in step S5, the sintering temperature is 500-1000° C., the sintering time is 6-14 hours, and the inert atmosphere is nitrogen.

[0019] According to one aspect of the embodiments of the present invention, the mass ratio of the resin-based asphalt to iron phosphate is 100:1 to 100:10.

[0020] Based on a general concept of the invention, an embodiment of the present invention further provides a high-density long-cycle lithium iron phosphate positive electrode material obtained by the above-mentioned preparation method.

[0021] Another object of an embodiment of the present invention is to provide an application of a high-density long-cycle lithium iron phosphate positive electrode material obtained by the above-mentioned preparation method in a lithium-ion battery.

[0022] The above scheme of the present invention has the following beneficial effects:

[0023] The present invention adopts resin-based asphalt with a β-resin content of 45%-55% as the carbon source. Since the β-resin has good bonding strength, a hard carbon and a soft carbon structure are formed during the sintering process, which can be evenly coated on the outer surface of the lithium iron phosphate material to form a stable core-shell structure. The prepared positive electrode material has a high compaction density, the formed coating layer is uniform and dense, and the cycle performance and rate performance are improved. DETAILED DESCRIPTION

[0024] In order to make the technical problems to be solved, technical solutions and advantages of the present invention more clear, they are described in detail below in conjunction with specific embodiments.

[0025] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0026] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0027] In view of the existing problems, the present invention provides a method for preparing a high-density long-cycle lithium iron phosphate positive electrode material, comprising the following steps:

[0028] S1: iron phosphate and lithium carbonate are mixed with water and sand-milled to obtain slurry;

[0029] S2: taking resin-based asphalt and adding it to ethanol solvent, heating and stirring to dissolve, to obtain an asphalt solution;

[0030] S3: adding the slurry to the asphalt solution and performing sand milling to obtain a mixed solution;

[0031] S4: spray drying the mixed solution to obtain a positive electrode material precursor;

[0032] S5: Sintering the cathode material precursor at high temperature under the protection of an inert atmosphere, and then crushing it after cooling to room temperature to obtain the cathode material precursor.

[0033] According to one aspect of the embodiment of the present invention, in step S1, the particle size D50 after sand grinding is 0.8-1.2 μm.

[0034] According to one aspect of the embodiment of the present invention, in step S2, the heating temperature is 45-80°C and the time is 2-8h.

[0035] According to one aspect of the embodiment of the present invention, in step S2, the β resin content of the resin-based asphalt is 45% to 55%.

[0036] According to one aspect of the embodiment of the present invention, in step S3, the particle size D50 after sand grinding is 0.6-1.0 μm.

[0037] According to one aspect of the embodiment of the present invention, in step S4, the spray drying temperature is 90-250° C. and the time is 4-5 hours.

[0038] According to one aspect of the embodiment of the present invention, in step S5, the sintering temperature is 500-1000° C., the sintering time is 6-14 hours, and the inert atmosphere is nitrogen.

[0039] According to one aspect of the embodiments of the present invention, the mass ratio of the resin-based asphalt to iron phosphate is 100:1 to 100:10.

[0040] Based on a general concept of the invention, an embodiment of the present invention further provides a high-density long-cycle lithium iron phosphate positive electrode material obtained by the above-mentioned preparation method.

[0041] The following will describe the invention through specific embodiments.

[0042] Example 1

[0043] A method for preparing a high-density long-cycle lithium iron phosphate material comprises the following steps:

[0044] (1) Iron phosphate and lithium carbonate are mixed in water to obtain a slurry, which is then sand-milled for the first time. The particle size D50 after sand-milling is 0.8 μm.

[0045] (2) Add the resin-based asphalt into the ethanol solvent, stir and dissolve it, and heat it to 45°C for 8 hours.

[0046] (3) The asphalt solution prepared in step 2 is added to the slurry prepared in step 1, and the sand milling is continued. The particle size D50 after sand milling is 0.6 μm.

[0047] (4) Spray drying

[0048] (5) Under N2 atmosphere protection, the mixture was sintered at 500°C for 14 h, cooled to room temperature, and crushed into fine powder to obtain a high-density long-cycle lithium iron phosphate material.

[0049] The beta resin content of the resin-based asphalt is 45%; the mass ratio of the resin-based asphalt to iron phosphate is 100:1.

[0050] Example 2

[0051] The difference is that the β resin content of the resin-based asphalt is 50%, and the other parameters and steps are the same as Example 1.

[0052] Example 3

[0053] The difference is that the β resin content of the resin-based asphalt is 55%, and the other parameters and steps are the same as Example 1.

[0054] Example 4

[0055] The difference is that the mass ratio of resin-based asphalt to iron phosphate is 100:10, and other parameters and steps are the same as Example 1.

[0056] Example 5

[0057] The difference is that the mass ratio of resin-based asphalt to iron phosphate is 100:5, and the other parameters and steps are the same as Example 1.

[0058] Comparative Example 1

[0059] The difference is that the β resin content of the resin-based asphalt is 35%, and the other parameters and steps are the same as Example 1.

[0060] Comparative Example 2

[0061] The difference is that the β resin content of the resin-based asphalt is 65%, and the other parameters and steps are the same as Example 1.

[0062] The data in Table 1 were obtained by testing the lithium iron phosphate powders obtained in the above embodiments and comparative examples, and by testing lithium iron phosphate batteries made from the lithium iron phosphate materials obtained in the above embodiments and comparative examples.

[0063] Table 1

[0064]

[0065] It can be seen from Table 1 above that the present invention adopts resin-based asphalt with a β-resin content of 45%-55% as the carbon source. Since the β-resin has good bonding strength, hard carbon and soft carbon structures are formed during the sintering process, which are evenly coated on the outer surface of the lithium iron phosphate material to form a stable core-shell structure. The prepared positive electrode material has a high compaction density, the formed coating layer is uniform and dense, and the cycle performance and rate performance are improved.

[0066] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a high-density long-cycle lithium iron phosphate cathode material, characterized in that: The steps include: S1: iron phosphate and lithium carbonate are mixed with water and sand-milled to obtain slurry; S2: taking resin-based asphalt and adding it to ethanol solvent, heating and stirring to dissolve, to obtain an asphalt solution; S3: adding the slurry to the asphalt solution and performing sand milling to obtain a mixed solution; S4: spray drying the mixed solution to obtain a positive electrode material precursor; S5: Sintering the cathode material precursor at high temperature under the protection of an inert atmosphere, and then crushing it after cooling to room temperature to obtain the cathode material precursor.

2. The method for preparing a high-density long-cycle lithium iron phosphate positive electrode material according to claim 1, characterized in that: In step S1, the particle size D50 after sand grinding is 0.8-1.2 μm.

3. The method for preparing a high-density long-cycle lithium iron phosphate positive electrode material according to claim 1, characterized in that: In step S2, the heating temperature is 45-80°C and the time is 2-8h.

4. The method for preparing a high-density long-cycle lithium iron phosphate cathode material according to claim 1, characterized in that: In step S2, the β resin content of the resin-based asphalt is between 45% and 55%.

5. The method for preparing a high-density long-cycle lithium iron phosphate cathode material according to claim 1, characterized in that: In step S3, the particle size D50 after sand grinding is 0.6-1.0 μm.

6. The method for preparing a high-density long-cycle lithium iron phosphate cathode material according to claim 1, characterized in that: In step S4, the spray drying temperature is 90 to 250° C. and the time is 4 to 5 hours.

7. The method for preparing a high-densification-rate long-cycle lithium iron phosphate positive electrode material according to claim 1, characterized in that: In step S5, the sintering temperature is 500-1000° C., the sintering time is 6-14 hours, and the inert atmosphere is nitrogen.

8. The method for preparing a high-density long-cycle lithium iron phosphate cathode material according to claim 1, characterized in that: The mass ratio of the resin-based asphalt to iron phosphate is 100:1 to 100:

10.

9. A high-density-rate long-cycle lithium iron phosphate positive electrode material obtained by the preparation method according to any one of claims 1 to 8.

10. Use of a high-density long-cycle lithium iron phosphate cathode material obtained by the preparation method according to any one of claims 1 to 8 in a lithium-ion battery.