Coal gasification fine slag-based negative electrode material as well as preparation method and application thereof

By using coal gasified fine slag to prepare activated carbon materials with porous structures, the problems of poor electrochemical performance and high modification cost of existing coal-based anode materials are solved, and high capacity, low cost and environmentally friendly battery anode materials are realized, which promotes the Commercial application of sodium ion batteries.

CN119008938APending Publication Date: 2024-11-22YULIN UNIVERSITY +1

Patent Information

Application Number
CN202411023889.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The electrochemical performance of existing coal-based anode materials is poor and the modification cost is high, which limits the development of sodium ion batteries and large-scale production.

Method used

Using solid phase waste from the coal gasification industry - coal gasified fine slag as raw material, the activated coal gasified fine slag-based negative electrode material with porous structure is prepared through ball milling, pickling, hydrofluoro pickling, and high-temperature activation treatment to remove metal oxidation and silicate impurities to improve the content and electrochemical properties of carbon materials.

Benefits of technology

The prepared coal gasified fine slag-based anode material has high specific capacity, high conductivity, good stability and low cost. The porous structure improves the electrochemical performance and ion transmission efficiency of the battery, and reduces the cost of the battery and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008938A_ABST
    Figure CN119008938A_ABST
Patent Text Reader

Abstract

The invention relates to a coal gasification fine slag-based negative electrode material and a preparation method and application thereof, and the preparation method comprises the following steps: 1) carrying out ball milling and screening on coal gasification fine slag to obtain pretreated coal gasification fine slag; 2) performing hydrochloric acid water bath treatment on the pretreated fine coal gasification slag to obtain fine coal gasification slag without metal oxide; (3) washing the fine coal gasification slag from which the metal oxides are to be removed by using deionized water until a washing solution is neutral, carrying out hydrofluoric acid water bath treatment, and washing until the washing solution is neutral, so as to obtain carbon residues; and 4) mixing the residual carbon and potassium hydroxide according to a certain proportion, putting the mixture into a tubular furnace, performing high-temperature activation treatment in a nitrogen atmosphere, cooling, washing, performing suction filtration, and drying to obtain activated coal gasification fine slag residual carbon, namely the coal gasification fine slag-based negative electrode material. The prepared negative electrode material is high in carbon content and has a porous structure. The method has simple process steps and can significantly improve the electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of negative electrode materials, and in particular to a coal gasification fine slag-based negative electrode material and a preparation method and application thereof. Background Art

[0002] Due to the small theoretical capacity of graphite, its use in high-power environments is greatly limited. The repeated insertion and extraction of lithium ions during the cycle will cause the volume of the material to change. Under low-pressure conditions, the graphite negative electrode and the electrolyte will produce a chemical reaction. Therefore, it is urgent to develop a lithium-ion battery negative electrode material with high capacity, high cycle stability and high safety.

[0003] As a new type of secondary battery, sodium-ion batteries have the advantages of low cost, abundant resources and wide distribution. In addition, the redox reaction has strong reversibility of electron gain and loss, and the working potential of the sodium-ion negative electrode is slightly higher than that of lithium-ion batteries. It is not easy to form metal dendrites and has higher safety. In the process of large-scale energy storage, people have higher requirements for cost and safety, so sodium-ion batteries are receiving more and more attention in the field of electrochemistry.

[0004] In 2021, CATL took the lead in launching the first generation of sodium-ion batteries, with a single cell energy density of 160WhKg -1 , setting a new global record. Although sodium-ion batteries are about to be industrialized, their poor energy storage performance and low energy density have limited their development.

[0005] The patent application document with application number 202210374215.4 discloses a method for preparing coal-based materials as negative electrode materials for sodium ion batteries. It is prepared through two simple steps of mixing and carbonization. During the carbonization process, the volatilization of impurities causes the material to form many pores, which is conducive to the diffusion of sodium ions; in the process of surface coating with amorphous carbon, the specific surface area of ​​the material is reduced. The synergistic effect of the two greatly improves the capacity and initial efficiency of carbon negative electrode materials. However, the volatilized aromatic gases during the carbonization process of coal-based materials are toxic and harmful to organisms, and the consistency of surface coating is difficult to guarantee, which is not suitable for large-scale production.

[0006] The patent application document with application number 202211706329.0 discloses a method for preparing coal-based materials as negative electrode materials for sodium ion batteries, wherein a precursor material is obtained by gas phase hybridization coating treatment, and then a hard carbon material is obtained by high temperature carbonization treatment, thereby improving the sodium storage capacity and the first coulombic efficiency. However, its defects are that the gas phase doping process is costly, the coating effect is poor, and the improvement of electrochemical performance is not significant.

[0007] In summary, the defects of the existing technology are that the electrochemical performance of the coal-based negative electrode is poor and the modification cost is high, which is not conducive to large-scale production. Summary of the invention

[0008] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to propose a coal gasification fine slag-based negative electrode material and its preparation method and application. The preparation method uses the solid waste of the coal gasification industry, namely, coal gasification slag stone, as raw material to prepare the negative electrode material, which is not only low in cost and abundant in source, but also the prepared negative electrode material has a high carbon content and a porous structure, which can significantly improve the electrochemical performance.

[0009] In order to achieve the above object, the technical solution adopted by the present invention is:

[0010] A coal gasification fine slag-based negative electrode material, which is activated coal gasification fine slag carbon residue, wherein the activated coal gasification fine slag carbon residue is in a granular and flaky structure, the granular surface has a porous structure, the porous structure size is 2-10um, and the granular particles are loose in texture and are agglomerated from small particles;

[0011] The carbon material atomic structure of the activated coal gasification fine slag residual carbon is a few-layer graphene-like state, the few-layer graphene-like state is disorderly arranged, and the carbon material atomic structure surface is curved and wrinkled.

[0012] A method for preparing a coal gasification fine slag-based negative electrode material comprises the following steps:

[0013] Step 1) Raw material pretreatment:

[0014] After ball milling and screening the coal gasification fine slag, the pretreated coal gasification fine slag is obtained;

[0015] Step 2) Metal oxide removal treatment:

[0016] The pretreated coal gasification fine slag is subjected to hydrochloric acid water bath treatment to obtain coal gasification fine slag with metal oxides removed;

[0017] Step 3) Silicate removal treatment:

[0018] The coal gasification slag fine residue from which metal oxides are to be removed is washed with deionized water until the washing liquid is neutral, and then treated with hydrofluoric acid water bath and washed until the washing liquid is neutral to obtain residual carbon;

[0019] Step 4) High temperature activation treatment:

[0020] After the residual carbon and potassium hydroxide are mixed in a certain proportion, the mixture is placed in a tubular furnace and subjected to high-temperature activation treatment in a nitrogen atmosphere. After cooling, the mixture is washed, filtered, and dried to obtain activated coal gasification fine slag residual carbon, i.e., coal gasification fine slag-based negative electrode material.

[0021] In the step 1) of pretreatment, the ball-to-material ratio of ball milling is 10-20:1, the rotation speed of ball milling is 150-200 rpm, the ball milling time is 0.5-1 hour, and the pretreated coal gasification fine slag of 50-75 μm is screened for use. The carbon content is highest in this particle size range.

[0022] In the step 2), the coal gasification fine slag obtained in the step 1) is treated with hydrochloric acid having a mass concentration of 10% under stirring conditions for 2 to 6 hours at a temperature of 60 to 80° C., wherein the solid-liquid mass ratio is 1:5 to 1:20; the purpose of this is to fully remove the metal oxide impurities remaining in the raw material.

[0023] In the step 3), the gasified fine slag treated in step 2) is treated with hydrofluoric acid with a mass concentration of 8% under stirring conditions for 2 to 6 hours at a temperature of 60 to 80° C., wherein the solid-liquid mass ratio is 1:5 to 1:10, so as to fully remove the silicate impurities remaining in the raw material.

[0024] In the step 4), the residual carbon and potassium hydroxide are stirred for 2-12 hours to be fully mixed, the mass ratio of the two is 1:0.5-1:5, the heating rate is 10°C / min, the activation temperature is 600-1000°C, and the insulation time is 2-10 hours.

[0025] The coal gasification fine slag-based negative electrode material is used as an alkali metal ion battery negative electrode material. The porous structure of the carbon material atomic structure has abundant active sites and a semi-open crystal structure, and the porous structure has a large specific surface area, which is conducive to the embedding and extraction of alkali metal ions, thereby improving the electrochemical performance of the battery.

[0026] Beneficial effects of the present invention:

[0027] The coal gasification fine slag-based negative electrode material prepared by the present invention has the characteristics of high carbon content and porosity, which meets the characteristics of battery negative electrode materials. The carbon in the residual carbon of activated coal gasification fine slag as a negative electrode material has the advantages of high specific capacity, high conductivity, good stability and low cost. The porous structure can increase the surface area of ​​the material, improve the storage and release speed of the battery, and can also promote ion transmission and reduce the resistance in the ion transmission process.

[0028] The surface of the activated coal gasification fine slag carbon particles has a porous structure with a size of 2-10um, which is conducive to the embedding and extraction of alkali metal ions, thereby improving the electrochemical performance of the battery.

[0029] The present invention uses solid waste generated during the coal gasification process, namely coal gasification fine slag, as raw material, which not only helps to reduce the cost of lithium / sodium ion batteries, but also promotes the commercial application of sodium ion batteries.

[0030] The preparation method of the present invention comprises the following steps: 1) screening 50-75 μm pre-treated coal gasification fine slag, which has the highest carbon content.

[0031] The conditions of step 2) of the preparation method of the present invention are used to fully remove the metal oxide impurities remaining in the raw materials.

[0032] The conditions of step 3) of the preparation method of the present invention are used to fully remove the silicate impurities remaining in the raw materials.

[0033] In summary, the preparation method of the present invention uses a simple process to remove impurities to obtain a carbon source, and carbonizes the impurities to obtain the carbon source, thereby obtaining the coal gasification fine slag-based negative electrode material prepared by the present invention. At the same time, it provides a new idea for turning waste into treasure for the utilization of coal gasification fine slag, which can reduce environmental pollution, reduce carbon emissions, and promote green development. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is the SEM image of coal gasification fine slag-based negative electrode material.

[0035] Figure 2 TEM image of coal gasification slag negative electrode material.

[0036] Figure 3 This is the XRD pattern of Example 1.

[0037] Figure 4 The charge and discharge curves of the lithium ion half-cell of Example 1 at different cycle numbers at 0.5C are shown.

[0038] Figure 5 This is a graph showing the cycling performance of the lithium-ion half-cell of Example 1 at 0.5C.

[0039] Figure 6 The charge and discharge curves of the sodium ion half-cell of Example 2 at different cycle numbers at 0.5C. DETAILED DESCRIPTION

[0040] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0041] Embodiment 1:

[0042] Step 1): Mix the coal gasification fine slag and grinding balls at a ratio of 15:1, ball mill for 1 hour at a rotation speed of 200 rpm, and sieve with a 200-mesh sieve to obtain pretreated coal gasification fine slag with a particle size range of 50-75 μm;

[0043] Step 2): treating the pretreated coal gasification fine slag with a 10% hydrochloric acid solution at a solid-liquid mass ratio of 1:20, treating in a water bath at 80° C. for 6 hours, filtering, washing, and drying to obtain coal gasification fine slag with metal oxides removed;

[0044] Step 3): treating the coal gasification slag from which metal oxides have been removed with a hydrofluoric acid solution of 8% by mass concentration for a second time, with a solid-liquid mass ratio of 1:10, treating in a water bath at 80° C. for 6 hours, and obtaining the residual carbon after filtration, washing and drying;

[0045] Step 4): The residual carbon and potassium hydroxide are mixed in a mass ratio of 1:4, stirred for 12 hours, placed in a tube furnace, heated to 1000°C at a heating rate of 10°C / min under a nitrogen atmosphere, kept warm for 2 hours, cooled to room temperature, and washed in turn with 10% hydrochloric acid solution, anhydrous ethanol and deionized water to a neutral pH value, and dried to obtain an activated residual carbon material.

[0046] Step 5): Assemble a lithium-ion battery using the activated carbon residue material as the negative electrode active material and conduct an electrochemical performance test.

[0047] like Figure 3 As shown, it can be seen from the attached figure that all samples have two obvious peaks near 23° and 43°, which belong to the (0 0 2) and (1 0 0) crystal planes of graphite crystallites, respectively.

[0048] like Figure 4 As shown in the figure, it can be seen that the lithium-ion battery half-cell using the activated carbon residue negative electrode obtained 453mAh g in the first cycle. -1 After 100 cycles, it can still maintain 273mAh g -1 The discharge capacity.

[0049] like Figure 5 As shown in the figure, it can be seen that the battery can still maintain 175mAg after 120 cycles. -1 The capacity and coulombic efficiency are close to 100%, which shows that it is feasible to use coal gasification slag as negative electrode material for lithium-ion batteries.

[0050] The carbon material prepared in step 4) above was subjected to SEM test, and the results are shown in the attached figure. Figure 1 As shown, the activated carbon residue obtained is in the form of particles and flakes, and a porous structure can be clearly observed on the surface of the particles. The particles are loose in texture and are formed by the agglomeration of a large number of small particles. Therefore, they have a large specific surface area, which is conducive to the embedding and extraction of alkali metal ions, thereby improving the electrochemical performance of the battery.

[0051] The carbon material prepared in step 4) was further subjected to TEM test, and the results are shown in the attached figure. Figure 2From the TEM image, we can see that the atomic structure of the carbon material is a few-layer graphene-like state, with an overall disordered arrangement and curved and wrinkled atomic planes, which indicates that the carbon material has abundant active sites and a semi-open crystal structure, which is conducive to the embedding and extraction of alkali metal ions, thereby improving the electrochemical performance of the battery.

[0052] Embodiment 2:

[0053] Step 1) Mixing coal gasification fine slag and grinding balls at a ratio of 10:1, ball milling for 1 hour at a rotation speed of 200 rpm, and sieving with a 200-mesh sieve to obtain pretreated coal gasification fine slag with a particle size range of 50-75 μm;

[0054] Step 2) treating the pretreated coal gasification fine slag with a 10% hydrochloric acid solution at a solid-liquid mass ratio of 1:5, treating in a water bath at 60° C. for 2 hours, filtering, washing, and drying to obtain coal gasification fine slag with metal oxides removed;

[0055] Step 3) treating the coal gasification slag from which metal oxides have been removed with a hydrofluoric acid solution of 8% by mass concentration, with a solid-liquid mass ratio of 1:5, and treating in a water bath at 60° C. for 2 hours, and obtaining a carbon residue after filtration, washing, and drying;

[0056] Step 4) The residual carbon and potassium hydroxide are mixed in a mass ratio of 1:0.5, stirred for 2 hours, placed in a tube furnace, heated to 600°C at a heating rate of 10°C / min under a nitrogen atmosphere, kept warm for 2 hours, cooled to room temperature, and washed in sequence with 10% hydrochloric acid solution, anhydrous ethanol and deionized water to a neutral pH value, and dried to obtain an activated residual carbon material.

[0057] Step 5) Assembling a sodium ion battery using the activated carbon residue material as the negative electrode active material and conducting an electrochemical performance test.

[0058] like Figure 6 As shown in the figure, it can be seen that the sodium ion battery half-cell using activated carbon residue negative electrode obtained 103mAh g in the first cycle. -1 After 100 cycles, it can still maintain 73 mAh g -1 The discharge capacity.

[0059] Embodiment 3:

[0060] Step 1): Mix the coal gasification fine slag and grinding balls at a ratio of 20:1, ball mill for 1 hour at a rotation speed of 200 rpm, and sieve with a 200-mesh sieve to obtain pretreated coal gasification fine slag with a particle size range of 50-75 μm;

[0061] Step 2): treating the pretreated coal gasification fine slag with a 10% hydrochloric acid solution at a solid-liquid mass ratio of 1:20, treating in a water bath at 70° C. for 6 hours, filtering, washing, and drying to obtain coal gasification fine slag with metal oxides removed;

[0062] Step 3): treating the coal gasification slag from which metal oxides have been removed with a hydrofluoric acid solution of 8% by mass concentration for a second time, with a solid-liquid mass ratio of 1:10, and treating in a water bath at 70° C. for 6 hours, and obtaining the residual carbon after filtration, washing, and drying;

[0063] Step 4): The residual carbon and potassium hydroxide are mixed in a mass ratio of 1:4, stirred for 12 hours, placed in a tube furnace, heated to 700°C at a heating rate of 10°C / min under a nitrogen atmosphere, kept warm for 2 hours, cooled to room temperature, and washed in sequence with a 10% hydrochloric acid solution, anhydrous ethanol and deionized water to a neutral pH value, and dried to obtain an activated residual carbon material.

[0064] Embodiment 4:

[0065] Step 1): Mix the coal gasification fine slag and grinding balls at a ratio of 15:1, ball mill for 1 hour at a rotation speed of 200 rpm, and sieve with a 200-mesh sieve to obtain pretreated coal gasification fine slag with a particle size range of 50-75 μm;

[0066] Step 2): treating the pretreated coal gasification fine slag with a 10% hydrochloric acid solution at a solid-liquid mass ratio of 1:20, treating in a water bath at 65° C. for 6 hours, filtering, washing and drying to obtain coal gasification fine slag with metal oxides removed;

[0067] Step 3): treating the coal gasification slag from which metal oxides have been removed with a hydrofluoric acid solution of 8% by mass concentration for a second time, with a solid-liquid mass ratio of 1:10, treating in a water bath at 65° C. for 6 hours, and obtaining the residual carbon after filtration, washing and drying;

[0068] Step 4): Mix the residual carbon and potassium hydroxide in a mass ratio of 1:4, stir for 12 hours, place in a tubular furnace, heat at 650°C at a heating rate of 10°C / min in a nitrogen atmosphere, keep warm for 2 hours, cool to room temperature, wash with 10% hydrochloric acid solution, anhydrous ethanol and deionized water in turn until the pH value is neutral, and dry to obtain an activated residual carbon material. The coal gasification fine slag-based negative electrode material prepared by the present invention has a high carbon content and is porous, which meets the characteristics of battery negative electrode materials. The carbon in the activated coal gasification fine slag residual carbon as a negative electrode material has the advantages of high specific capacity, high conductivity, good stability and low cost. Porous materials can increase the surface area of ​​the material, improve the storage and release rate of the battery, and can also promote ion transmission and reduce resistance during ion transmission.

Claims

1. A coal gasification fine slag-based negative electrode material, characterized in that: The activated coal gasification fine slag carbon residue is in a granular and flaky structure, the granular surface has a porous structure, the porous structure size is 2-10um, the granular particles are loose in texture, and are agglomerated from small particles; The carbon material atomic structure of the activated coal gasification fine slag residual carbon is a few-layer graphene-like state, the few-layer graphene-like state is disorderly arranged, and the carbon material atomic structure surface is bent and wrinkled.

2. The method for preparing a coal gasification fine slag-based negative electrode material according to claim 1, characterized in that: The following steps are involved: Step 1) Raw material pretreatment: After ball milling and screening the coal gasification fine slag, the pretreated coal gasification fine slag is obtained; Step 2) Metal oxide removal treatment: The pretreated coal gasification fine slag is subjected to hydrochloric acid water bath treatment to obtain coal gasification fine slag with metal oxides removed; Step 3) Silicate removal treatment: The coal gasification slag fine residue from which metal oxides are to be removed is washed with deionized water until the washing liquid is neutral, and then treated with hydrofluoric acid water bath and washed until the washing liquid is neutral to obtain residual carbon; Step 4) High temperature activation treatment: After the residual carbon and potassium hydroxide are mixed in a certain proportion, the mixture is placed in a tubular furnace and subjected to high-temperature activation treatment in a nitrogen atmosphere. After cooling, the mixture is washed, filtered, and dried to obtain activated coal gasification fine slag residual carbon, i.e., coal gasification fine slag-based negative electrode material.

3. The method for preparing a coal gasification fine slag-based negative electrode material according to claim 2, characterized in that: In the step 1) of pretreatment, the ball-to-material ratio of ball milling is 10-20:1, the rotation speed of ball milling is 150-200 rpm, the ball milling time is 0.5-1 hour, and the pretreated coal gasification fine slag of 50-75 μm is screened for use.

4. The method for preparing a coal gasification fine slag-based negative electrode material according to claim 2, characterized in that: In the step 2), the coal gasification fine slag obtained in the step 1) is treated with 10% hydrochloric acid under stirring conditions for 2 to 6 hours at a temperature of 60 to 80° C., wherein the solid-liquid mass ratio is 1:5 to 1:

20.

5. The method for preparing a coal gasification fine slag-based negative electrode material according to claim 2, characterized in that: In the step 3), the gasified fine slag treated in step 2) is treated with hydrofluoric acid having a mass concentration of 8% under stirring conditions for 2 to 6 hours at a temperature of 60 to 80° C., wherein the solid-liquid mass ratio is 1:5 to 1:

10.

6. The method for preparing a coal gasification fine slag-based negative electrode material according to claim 2, characterized in that: In the step 4), the residual carbon and potassium hydroxide are stirred for 2-12 hours to be fully mixed, the mass ratio of the two is 1:0.5-1:5, the heating rate is 10°C / min, the activation temperature is 600-1000°C, and the insulation time is 2-10 hours.

7. The use of the coal gasification fine slag-based negative electrode material according to any one of claims 1 to 6, characterized in that: Coal gasification fine slag-based negative electrode materials are used as negative electrode materials for alkali metal ion batteries. The porous structure of the carbon material atomic structure has abundant active sites and a semi-open crystal structure, and the porous structure has a large specific surface area, which is conducive to the embedding and extraction of alkali metal ions, thereby improving the electrochemical performance of the battery.

Citation Information

Patent Citations

  • Preparation method of negative electrode material for sodium ion battery

    CN114709393A

  • Hard carbon material and preparation method and application thereof

    CN115744874A

Cited By

  • Preparation method of carbon-rich coal gasification slag-based iodine-doped C / SiOx composite lithium battery negative electrode material

    CN120136109A

  • Battery negative electrode material with coal gasification slag soft carbon-asphalt hard carbon core-shell structure and preparation method of battery negative electrode material