CAU-10-X series modified polybenzimidazole one-dimensional densified ionic solvent film as well as preparation method and application thereof

By combining polyphosphate sol-gel preparation and one-dimensional directional densification process and in-situ growth technology of metal organic frame materials, a CAU-10-X series modified polybenzimidazole one-dimensional densified ionic solvent film was prepared, and the solution was solved The balance between proton conductivity and vanadium ion transmittance in liquid flow batteries has achieved efficient ion selectivity and improved battery performance.

CN119009045APending Publication Date: 2024-11-22ZHEJIANG UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411106919.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The ion exchange membrane of existing flow batteries is too dense, resulting in a decrease in proton conductivity, or is too loose, resulting in a crossover of vanadium ions, reducing battery capacity and life. The traditional polybenzimidazole structure has problems such as poor solubility and low acid loading levels.

Method used

Using polyphosphate sol-gel preparation technology and one-dimensional directional densification process combined with in-situ growth technology of metal organic frame materials, CAU-10-X series modified polybenzimidazole one-dimensional densified ionic solvent film was prepared to form hundreds of The superposition structure of nanosheets improves proton conductivity and reduces vanadium ion transmittance.

Benefits of technology

It achieves high proton conductivity and excellent ion selectivity, significantly improving the Coulomb efficiency, voltage efficiency and energy efficiency of the battery, especially showing good operating performance under high current density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009045A_ABST
    Figure CN119009045A_ABST
Patent Text Reader

Abstract

The invention discloses a CAU-10-X series modified polybenzimidazole one-dimensional densified ionic solvent film as well as a preparation method and application thereof. The ionic solvent film is prepared from a gel type polybenzimidazole film with a loose network porous structure through a one-dimensional directional densification process and a CAU-10-X in-situ growth technology. The membrane is further densified on the basis of retaining a porous structure of a gel membrane and is uniformly loaded with a CAU-10-X layer through an in-situ growth strategy, and the ion selectivity is further improved by utilizing a special pore diameter structure of CAU-10-X; the ionic solvent membrane disclosed by the invention breaks through the restrictive relationship between proton conductivity and vanadium ion transmittance to a certain extent, can be applied to a flow battery, particularly shows excellent proton conductivity, ion selectivity, chemical stability and battery performance on an all-vanadium flow battery, can operate under relatively high current density, and has a wide application prospect. Good application prospects are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polymer ion solvent membrane that can be used for a liquid flow battery, and in particular to a CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane and a preparation method and application thereof. Background Art

[0002] With the continuous increase of global population and the booming industry, environmental pollution and global climate deterioration are becoming more and more serious. Countries around the world are vigorously developing and utilizing renewable energy. Since the currently large-scale renewable energy such as solar energy and wind energy are intermittent and volatile, they need to be combined with energy storage technology. Among all energy storage technologies, redox flow battery (RFB) has attracted more and more attention because it can accelerate the utilization of renewable energy by solving the problems of discontinuity, instability and uncontrollability.

[0003] Ion exchange membranes play the role of isolating electrolytes on both sides and conducting protons, and are key components that determine battery performance. If the flow battery separator is too dense, the proton conductivity will decrease, thereby reducing the battery utilization efficiency; while being too loose and porous will lead to serious vanadium ion crossover, greatly reducing the battery capacity and shortening the battery life. Commercial Nafion membranes are expensive, and most ions penetrate seriously into the membrane, resulting in a reduction in battery capacity. The molecular chains of the traditional polybenzimidazole (PBI) structure are tightly stacked, resulting in poor solubility, low swelling level, and low acid loading level, which limits the proton conductivity. It is difficult to significantly improve. The PBI ion solvent membrane prepared by the new sol-gel method uses polyphosphoric acid as a solvent, scrapes the polymer solution on the substrate, and completes the phase transformation process from solution (sol) to gel membrane (gel) through the process of hydrating polyphosphoric acid to phosphoric acid, and obtains a gel-type PBI membrane. The obtained gel-type membrane can greatly improve the absorption of ion solvents and greatly improve proton conductivity. However, the PBI gel membrane prepared in this way has a loose structure and serious electrolyte cross contamination. On this basis, the polybenzimidazole ion solvent membrane prepared by the new sol-gel method was subjected to one-dimensional directional densification, so that the membrane layers were shrunk and overlapped again, which can effectively reduce the vanadium ion permeability while ensuring a higher proton conductivity. However, there is still room for improvement in the vanadium barrier performance of the membrane.

[0004] Metal organic frameworks (MOFs) are one-dimensional, two-dimensional or three-dimensional network structures that are self-assembled by metal ions or clusters and organic ligands connected by coordination. They have a special pore structure and a suitable pore size that can achieve high ion selectivity. Combining the two is expected to solve the problem of balancing proton conductivity and vanadium ion permeability.

[0005] The present invention proposes to prepare a CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane by combining a polyphosphate sol-gel preparation process with a one-dimensional directional densification process and an MOF in-situ growth technology. The pore size of CAU-10-X is 0.15 to 0.7 nm, the hydration radius of protons is 0.2 nm, and the hydration radius of vanadium ions is 0.7 nm. The introduction of CAU-10-X particles can greatly improve the ion selectivity. Due to its unique morphological advantages, the membrane not only has a high vanadium ion screening ability, but also has a high acid doping level and can quickly absorb ionic solvents. In liquid flow batteries, it exhibits excellent ion selectivity and high proton conductivity, breaking through the restrictive relationship between proton conductivity and vanadium ion permeability to a certain extent, and can operate in a larger current density range, with good application prospects. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the present invention provides a CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane having both high vertical plane proton conductivity and excellent ion selectivity, as well as a preparation method and application thereof.

[0007] The ion solvent membrane of the present invention is prepared by a polyphosphoric acid sol-gel method, a one-dimensional directional densification process and an in-situ growth technology of a metal organic framework material. The ion solvent membrane prepared by the present invention greatly reduces the vanadium ion permeability while ensuring a certain proton conductivity, and has good application prospects in the fields of all-vanadium redox flow batteries and the like.

[0008] The technical solution of the present invention is as follows:

[0009] A CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane, which is composed of polybenzimidazole (PBI) and CAU-10-X series nanoparticles; the ion solvent membrane has a one-dimensional directional densified structure, and shrinks and stacks in the thickness direction to form a special morphology of hundreds of layers of nanosheets, and the CAU-10-X series nanoparticles are uniformly grown in the one-dimensional directional densified polybenzimidazole membrane matrix;

[0010] CAU-10-X series nanoparticles are aluminum-based metal organic framework materials, with aluminum as the metal center and isophthalic acid or its derivatives as organic ligands for self-assembly synthesis; in CAU-10-X series nanoparticles, -X represents one or more of the following functional groups: -H, -NH2, -OH, -CH3, -OCH3, -SO3, etc.; CAU-10-X series nanoparticles are irregular flakes with a molecular weight between 200 and 500;

[0011] The general structural formula of polybenzimidazole is as follows:

[0012]

[0013] The polybenzimidazole is a homopolymer or a random copolymer, n is the degree of polymerization, and is a positive integer of 340 to 500; the molecular weight of the polybenzimidazole is between 80,000 and 115,000;

[0014] -R- represents one or more of the following group structures:

[0015]

[0016] The CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane of the present invention has a pore size of 0.1-200 nm, a porosity of 25-70%, and a thickness of 5-60 μm.

[0017] A method for preparing a CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane comprises the following steps:

[0018] Step 1: Under an inert atmosphere, 3,3'-diaminobenzidine and dicarboxylic acid monomers are reacted in a solvent, polyphosphoric acid, to obtain a polybenzimidazole solution;

[0019] The molar ratio of 3,3'-diaminobenzidine to dicarboxylic acid monomer is 1:1, and the total mass fraction of the two monomers is 1-20wt% based on the total feed amount of the system;

[0020] The dicarboxylic acid monomer is selected from one or more of isophthalic acid, terephthalic acid, 2,5-dihydroxyterephthalic acid, and 2,5-dimethylbenzenesulfonic acid;

[0021] The preferred condensation reaction temperature is 185°C and the time is 36h;

[0022] Step 2: applying the polybenzimidazole solution obtained in step 1 on a glass substrate, completing the phase transformation from solution (sol) to gel film (gel) through the process of hydrating polyphosphoric acid to phosphoric acid, and obtaining a phosphoric acid-doped gel-type polybenzimidazole film;

[0023] The preferred scraping film thickness is 50 to 600 μm;

[0024] The temperature of the phase conversion process is 5 to 150°C, the relative humidity is 20 to 100%, and the phase conversion time is 10 to 30 hours;

[0025] Step 3: soaking the phosphoric acid-doped gel-type polybenzimidazole membrane obtained in step 2 in deionized water until it becomes neutral to remove the phosphoric acid doped in the membrane, and then using a one-dimensional directional densification process to shrink and overlap the membrane in the thickness direction to obtain a one-dimensional densified ion solvent membrane;

[0026] Soaking in deionized water was carried out at room temperature for ≥ 3 days, and the water was changed every 24 hours;

[0027] Specifically, the one-dimensional directional densification process refers to: using a porous plate to fix the membrane material so that its size in the plane direction remains unchanged, and only spontaneously shrinks and overlaps in the thickness direction to achieve one-dimensional directional densification, and finally drying to obtain a one-dimensional densified ion solvent membrane;

[0028] The purpose of drying is to completely evaporate the water in the film. Dry gas (such as air, nitrogen, etc.) can be used to accelerate the drying process. The thickness of the obtained one-dimensional densified ion solvent film is 5 to 60 μm.

[0029] Step 4: the one-dimensional densified ion solvent membrane obtained in step 3, aluminum salt, organic ligand and solvent are put into a reaction kettle, and a CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane is prepared by hydrothermal synthesis;

[0030] Aluminum salt, organic ligand, and solvent can be selected and proportioned according to the desired synthesized CAU-10-X, and CAU-10-X can be one or more of CAU-10-H, CAU-10-NH2, CAU-10-OH, CAU-10-CH3, CAU-10-OCH3, CAU-10-SO3, etc.;

[0031] Preferably, the aluminum salt is Al2(SO4)3·18H2O, the organic ligand is isophthalic acid, and the solvent is a mixed solvent of N,N-dimethylformamide (DMF) and water;

[0032] The reaction temperature of the hydrothermal synthesis is 100-160°C, and the reaction time is 6-48h.

[0033] The CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane of the present invention can be used in liquid flow batteries, including: all-vanadium liquid flow batteries, zinc / cerium liquid flow batteries, vanadium / iron liquid flow batteries or iron / chromium liquid flow batteries.

[0034] The specific application methods are as follows:

[0035] Carbon felt electrodes and CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membranes were assembled to obtain membrane electrode assemblies (MEAs). The obtained MEAs were installed in a flow battery single cell test device and charged and discharged at 25°C to measure the coulombic efficiency, voltage efficiency and energy efficiency of the battery at different current densities.

[0036] The CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane should be pre-doped with acid solution, and the doped acid solution is selected from one or more of sulfuric acid solution, hydrochloric acid solution, methanesulfonic acid solution, etc., and the hydrogen ion concentration in the doped acid solution does not exceed 6 mol / L;

[0037] The ionic solvent membrane can show a transmembrane proton conductivity of no less than 50 mS / cm in 3 mol / L sulfuric acid, and can reduce the vanadium ion permeability to 5×10 -9 cm 2 / s or less;

[0038] When the ion solvent membrane is applied to all-vanadium redox flow batteries, it can 2 It has a coulombic efficiency of more than 95%, a voltage efficiency of more than 55%, and an energy efficiency of 55% or higher at a current density of .

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) The CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane prepared by the present invention is a structure composed of hundreds of layers of nanosheets, which is conducive to the rapid absorption and storage of acid or other ion solutions, avoiding the problems of low liquid holding capacity and low ion transmission capacity existing in traditional dense membranes.

[0041] (2) The CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane prepared by the present invention is formed by the CAU-10-X in-situ growth technology. On the basis of forming a nanosheet structure with hundreds of layers of tightly stacked layers, CAU-10-X particles with a special pore structure are introduced, which further reduces the ion transmembrane permeability and alleviates the phenomenon of ion interpenetration on both sides of the solution when conventional porous membranes are used. At the same time, it solves the problem of poor compatibility and agglomeration between MOF materials and polybenzimidazole materials, and can be applied to liquid flow batteries.

[0042] (3) The CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane prepared by the present invention has high vertical plane proton conductivity and excellent battery charge and discharge performance. While ensuring high proton conductivity, it can significantly reduce the vanadium ion permeability; it can be 20-400mA / cm 2 The wide current density range, especially at 400 mA / cm 2 Even at high current density, it can still maintain 99% coulombic efficiency, 58% voltage efficiency and 57% energy efficiency.

[0043] (4) The present invention broadens the types and application scope of membrane materials used in liquid flow battery technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 : SEM image of CAU-10(Al) prepared in Example 1.

[0045] Figure 2 : Electron micrograph of the one-dimensional densified ion solvent membrane of polybenzimidazole modified by CAU-10 prepared in Example 1; A: Plane electron micrograph of the one-dimensional densified ion solvent membrane of polybenzimidazole modified by CAU-10; B: Cross-sectional electron micrograph of the one-dimensional densified ion solvent membrane of polybenzimidazole modified by CAU-10.

[0046] Figure 3 : Performance diagram of single cell tests of some embodiments and comparative examples.

[0047] Figure 4 : Comparison of proton conductivity and ion selectivity of some embodiments and comparative examples. DETAILED DESCRIPTION

[0048] For ease of understanding of the present invention, the present invention will be more fully described in conjunction with the following examples. However, the present invention can be implemented in many different forms, and protection scope is not limited to the embodiments described herein. In addition, for those skilled in the art, without departing from the essence and scope of the present invention, the various modifications or improvements of the material composition and the dosage in these embodiments all belong to the scope of protection claimed in the present invention.

[0049] Comparative Example 1:

[0050] Use m-PBI (commercial membrane) provided by PBIPerformance, USA, to prepare ion solvent membrane, and apply it to the all-vanadium liquid flow battery device to test its performance. The specific steps are as follows:

[0051] The m-PBI (commercial membrane) was immersed in a 3 mol / L sulfuric acid solution and treated at 25°C for 48 h to obtain an m-PBI ion solvent membrane;

[0052] The m-PBI ion solvent membrane is used as an electrolyte membrane in an all-vanadium redox flow battery device.

[0053] The carbon felt electrode purchased from SGL Special Graphite (Shanghai) Co., Ltd. was used, and the membrane effective area was 4 cm 2 , the membrane was clamped in the flow battery fixture. The proton conductivity test was performed at 25 °C.

[0054] The m-PBI ion solvent membrane was placed in an H-type electrolytic cell device filled with 1.5M VOSO4 / 3M H2SO4 and 1.5M MgSO4 / 3M H2SO4 to evaluate the absorbance change of the MgSO4 side at different times to evaluate the VO 2+ Ion permeability.

[0055] The m-PBI ion solvent membrane obtained in Comparative Example 1 was analyzed and tested:

[0056] Acid doping level: After doping with 3 mol / L H2SO4 solution at 25°C, the H2SO4 doping level in the membrane is: 30wt%

[0057] Proton conductivity (doped with 3 mol / L H2SO4 solution): 25°C conductivity: 0.008S / cm

[0058] Vanadium ion transmittance: 25℃VO 2+ Ion permeability: 2.53x10 -11 cm 2 / s

[0059] Comparative Example 2:

[0060] Use DuPont Nafion115 membrane and apply it to the all-vanadium liquid flow battery device to test its performance. The specific steps are as follows:

[0061] (1) The Nafion 115 membrane was immersed in a 5 wt.% hydrogen peroxide solution and treated at 80°C for 1 hour. The membrane was then repeatedly rinsed with deionized water and immersed in deionized water at 80°C for 1 hour.

[0062] (2) The treated Nafion 115 membrane was immersed in a 0.5 mol / L sulfuric acid solution and treated at 80°C for 5 h. The membrane was then repeatedly rinsed with deionized water. The membrane was immersed in deionized water and treated at 80°C for 5 h. The membrane was then immersed in a 3 mol / L sulfuric acid solution and treated at 25°C for 72 h.

[0063] (2) Nafion 115 membrane is used as electrolyte membrane in all-vanadium liquid flow battery device;

[0064] The proton conductivity test method of Nafion115 membrane is consistent with that of Comparative Example 1.

[0065] The test method of Nafion115 vanadium ion transmittance is consistent with that of Comparative Example 1.

[0066] The Nafion 115 membrane obtained in Comparative Example 2 was analyzed and tested:

[0067] Acid doping level: After doping with 3 mol / L H2SO4 solution at 25°C, the H2SO4 doping level in the membrane is 1.6 wt%

[0068] Proton conductivity (doped with 3 mol / L H2SO4 solution): 25°C conductivity: 0.07S / cm

[0069] Vanadium ion transmittance: 25℃VO 2+Ion permeability: 5.15x10 -7 cm 2 / s

[0070] Embodiment 1:

[0071] (1) Add 3,3-diaminobenzidine (2.7855 g, 0.0130 mol) and terephthalic acid (2.1611 g, 0.0130 mol) to a three-necked reaction bottle equipped with a mechanical stirrer, use polyphosphoric acid (160 mL) as solvent, the monomer content is 3 wt %, and react at 185° C. for 36 h under the protection of nitrogen flow until the polymer solution is sufficiently viscous;

[0072] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion, the temperature of the phase inversion process is 30° C., the relative humidity is 50%, and the phase inversion time is 24 h. Since the polyphosphoric acid is naturally hydrolyzed and converted into phosphoric acid, a phosphoric acid-doped gel-state polybenzimidazole ion solvent membrane is prepared through a solution-gel phase transition;

[0073] (3) The obtained membrane was soaked in deionized water to remove the phosphoric acid contained in the membrane, and a one-dimensional densified polybenzimidazole ion solvent membrane with a thickness of 25 μm was prepared by fixing the plane direction of the gel-state polybenzimidazole ion solvent membrane and performing directional shrinkage and lamination treatment only in thickness.

[0074] (4) According to the molar ratio of the reactants, n(Al 3+ ):n(isophthalic acid)=1:1, the solvent volume ratio is V DMF :V H2O =1:4, weigh Al2(SO4)3·18H2O (1.6 g, 0.0024 mol) and isophthalic acid (0.4 g, 0.0024 mol), and dissolve them in a mixed solvent (50 mL) of DMF and water, transfer the solution and the prepared one-dimensional densified polybenzimidazole ion solvent membrane to a hydrothermal synthesis reactor, and perform hydrothermal synthesis at 135°C for 12 h. After cooling, wash with DMF and deionized water in turn to prepare a CAU-10 modified polybenzimidazole one-dimensional densified ion solvent membrane.

[0075] The CAU-10 modified one-dimensional densified membrane obtained in Example 1 was analyzed and tested:

[0076] Acid doping level: After doping with 3 mol / L H2SO4 solution at 25°C, the H2SO4 doping level in the membrane is: 65wt%

[0077] Proton conductivity (doped with 3 mol / L H2SO4 solution): 25°C conductivity: 0.05S / cm

[0078] Vanadium ion transmittance: 25℃VO2+ Ion permeability: 3.15x10 -9 cm 2 / s

[0079] Embodiment 2:

[0080] (1) Add 3,3-diaminobenzidine (2.7855 g, 0.0130 mol) and terephthalic acid (2.1611 g, 0.0130 mol) to a three-necked reaction bottle equipped with a mechanical stirrer, use polyphosphoric acid (160 mL) as solvent, the monomer content is 3 wt %, and react at 185° C. for 36 h under the protection of nitrogen flow until the polymer solution is sufficiently viscous;

[0081] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion, the temperature of the phase inversion process is 30° C., the relative humidity is 50%, and the phase inversion time is 24 h. Since the polyphosphoric acid is naturally hydrolyzed and converted into phosphoric acid, a phosphoric acid-doped gel-state polybenzimidazole ion solvent membrane is prepared through a solution-gel phase transition;

[0082] (3) The obtained membrane was soaked in deionized water to remove the phosphoric acid contained in the membrane, and a one-dimensional densified polybenzimidazole ion solvent membrane with a thickness of 25 μm was prepared by fixing the plane direction of the gel-state polybenzimidazole ion solvent membrane and performing directional shrinkage and lamination treatment only in thickness.

[0083] (4) According to the molar ratio of the reactants, n(Al 3+ ):n(isophthalic acid)=1:1, the solvent volume ratio is V DMF :V H2O =1:4, weigh Al2(SO4)3·18H2O (0.8g, 0.0012mol) and isophthalic acid (0.2g, 0.0012mol), and dissolve them in a mixed solvent (50mL) of DMF and water, transfer the solution and the prepared one-dimensional densified polybenzimidazole ion solvent membrane to a hydrothermal synthesis reactor, and hydrothermally synthesize at 135℃ for 12h. After cooling, wash with DMF and deionized water in turn to prepare a CAU-10 modified polybenzimidazole one-dimensional densified ion solvent membrane.

[0084] The CAU-10 modified polybenzimidazole one-dimensional densified ion solvent membrane obtained in Example 2 was analyzed and tested:

[0085] Acid doping level: After doping with 3 mol / L H2SO4 solution at 25°C, the H2SO4 doping level in the membrane is: 60wt%

[0086] Proton conductivity (doped with 3 mol / L H2SO4 solution): 25°C conductivity: 0.056S / cm

[0087] Vanadium ion transmittance: 25℃VO 2+ Ion permeability: 1.42x10 -9 cm 2 / s

[0088] Embodiment 3:

[0089] (1) Add 3,3-diaminobenzidine (2.7855 g, 0.0130 mol) and terephthalic acid (2.1611 g, 0.0130 mol) to a three-necked reaction bottle equipped with a mechanical stirrer, use polyphosphoric acid (160 mL) as solvent, the monomer content is 3 wt %, and react at 185° C. for 36 h under the protection of nitrogen flow until the polymer solution is sufficiently viscous;

[0090] (2) scraping the obtained polymer solution onto a glass substrate for phase inversion, the temperature of the phase inversion process is 30° C., the relative humidity is 50%, and the phase inversion time is 24 h. Since the polyphosphoric acid is naturally hydrolyzed and converted into phosphoric acid, a phosphoric acid-doped gel-state polybenzimidazole ion solvent membrane is prepared through a solution-gel phase transition;

[0091] (3) The obtained membrane was soaked in deionized water to remove the phosphoric acid contained in the membrane, and a one-dimensional densified polybenzimidazole ion solvent membrane with a thickness of 25 μm was prepared by fixing the plane direction of the gel-state polybenzimidazole ion solvent membrane and performing directional shrinkage and lamination treatment only in thickness.

[0092] (4) According to the molar ratio of the reactants, n(Al 3+ ):n(isophthalic acid)=1:1, the solvent volume ratio is V DMF :V H2O =1:4, weigh Al2(SO4)3·18H2O (0.4g, 0.0006mol) and isophthalic acid (0.1g, 0.0006mol), and dissolve them in a mixed solvent (50mL) of DMF and water, transfer the solution and the prepared one-dimensional densified polybenzimidazole ion solvent membrane to a hydrothermal synthesis reactor, and hydrothermally synthesize at 135℃ for 12h. After cooling, wash with DMF and deionized water in turn to prepare a CAU-10 modified polybenzimidazole one-dimensional densified ion solvent membrane.

[0093] The CAU-10 modified polybenzimidazole one-dimensional densified ion solvent membrane obtained in Example 3 was analyzed and tested:

[0094] Acid doping level: After doping with 3 mol / L H2SO4 solution at 25°C, the H2SO4 doping level in the membrane is 62wt%

[0095] Proton conductivity (doped with 3 mol / L H2SO4 solution): 25°C conductivity: 0.058 S / cm

[0096] Vanadium ion transmittance: 25℃VO 2+ Ion permeability: 2.13x10 -9 cm 2 / s

[0097] The CAU-10 modified polybenzimidazole one-dimensional densified ion solvent membrane obtained in Example 1 was installed in the all-vanadium redox flow battery device. The test results are as follows: Figure 3 .

[0098] Table 1 Proton conductivity and vanadium ion permeability test of the embodiment and the comparative example

[0099]

Claims

1. A CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane, It is characterized in that It is composed of polybenzimidazole and CAU-10-X series nanoparticles; the ion solvent membrane has a one-dimensional directional densified structure, and shrinks and stacks in the thickness direction to form a special morphology of hundreds of layers of nanosheets, and the CAU-10-X series nanoparticles are uniformly grown in the one-dimensional directional densified polybenzimidazole membrane matrix; CAU-10-X series nanoparticles are aluminum-based metal organic framework materials. In CAU-10-X series nanoparticles, -X represents one or more of the following functional groups: -H, -NH 2 、-OH、-CH 3 、-OCH 3 、-SO 3 ; The general structural formula of polybenzimidazole is as follows: Polybenzimidazole is a homopolymer or a random copolymer, and n is a degree of polymerization, which is a positive integer ranging from 340 to 500; -R- represents one or more of the following group structures:

2. The CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane as claimed in claim 1, It is characterized in that The CAU-10-X series nanoparticles are in irregular flake shape with a molecular weight between 200 and 500; the molecular weight of polybenzimidazole is between 80,000 and 115,000.

3. The CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane as claimed in claim 1, It is characterized in that The ion solvent membrane has a pore size of 0.1 to 200 nm, a porosity of 25 to 70%, and a thickness of 5 to 60 μm.

4. The method for preparing the CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane as claimed in claim 1, It is characterized in that The following steps are involved: Step 1: Under an inert atmosphere, 3,3'-diaminobenzidine and dicarboxylic acid monomers are reacted in a solvent, polyphosphoric acid, to obtain a polybenzimidazole solution; The dicarboxylic acid monomer is selected from one or more of isophthalic acid, terephthalic acid, 2,5-dihydroxyterephthalic acid, and 2,5-dimethylbenzenesulfonic acid; Step 2: applying the polybenzimidazole solution obtained in step 1 on a glass substrate by scraping, completing the phase transformation from solution to gel film through the process of hydrating polyphosphoric acid to phosphoric acid, and obtaining a phosphoric acid-doped gel-type polybenzimidazole film; Step 3: soaking the phosphoric acid-doped gel-type polybenzimidazole membrane obtained in step 2 in deionized water until it becomes neutral to remove the phosphoric acid doped in the membrane, and then using a one-dimensional directional densification process to shrink and overlap the membrane in the thickness direction to obtain a one-dimensional densified ion solvent membrane; Step 4: the one-dimensional densified ion solvent membrane obtained in step 3, aluminum salt, organic ligand and solvent are put into a reaction kettle, and a CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane is prepared by hydrothermal synthesis; Aluminum salt, organic ligand, and solvent are selected and proportioned according to the desired synthesized CAU-10-X, where CAU-10-X is CAU-10-H, CAU-10-NH 2 、CAU-10-OH、CAU-10-CH 3 、CAU-10-OCH 3 、CAU-10-SO 3 One or more of .

5. The preparation method according to claim 4, It is characterized in that In step 1, the molar ratio of 3,3'-diaminobenzidine to the dicarboxylic acid monomer is 1:

1.

6. The preparation method according to claim 4, It is characterized in that In step 1, the condensation reaction temperature is 185° C. and the time is 36 h.

7. The preparation method according to claim 4, It is characterized in that In step 2, the temperature of the phase conversion process is 5 to 150° C., the relative humidity is 20 to 100%, and the phase conversion time is 10 to 30 hours.

8. The preparation method according to claim 4, It is characterized in that In step 3, the one-dimensional directional densification process refers to: using a porous plate to fix the membrane material so that its size in the plane direction remains unchanged, and it only shrinks and overlaps spontaneously in the thickness direction to achieve one-dimensional directional densification, and finally drying to obtain a one-dimensional densified ion solvent membrane.

9. The preparation method according to claim 4, It is characterized in that In step 4, the aluminum salt is Al 2 (SO 4 ) 3 18H 2 O, the organic ligand is isophthalic acid, and the solvent is a mixed solvent of N,N-dimethylformamide and water; the reaction temperature of the hydrothermal synthesis is 100-160° C., and the reaction time is 6-48 hours.

10. Application of the CAU-10-X series modified polybenzimidazole one-dimensional densified ion solvent membrane as claimed in claim 1 in a liquid flow battery.

Citation Information

Cited By

  • Enhanced polybenzimidazole ion solvated composite membrane as well as preparation and application thereof

    CN119823380A