Preparation method of Li6. 28La3Zr2Al0. 24O12 nano solid electrolytic material

Nano-scale Li6.28La3Zr2Al0.24O12 solid electrolyte is prepared through template induction and high-temperature calcination technology, which solves the thermal instability and safety hazards of liquid electrolytes in lithium-ion batteries, and realizes the lithium-ion battery electrolyte with high energy density and long cycle life. , significantly improves the safety and performance of the battery.

CN119009081APending Publication Date: 2024-11-22NORTHEAST NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411142559.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Due to the thermal instability, electrochemical instability and safety risks of liquid electrolytes, existing lithium-ion batteries are difficult to meet the needs of high energy density, long cycle life and low cost, especially the risks of fire and explosion.

Method used

The nanoscale Li6.28La3Zr2Al0.24O12 solid electrolyte material was prepared by template induction and high-temperature calcination technology. Through the preparation of a variety of salt mixtures, ultrasonic reaction, freeze-drying and high-temperature calcination, garnet bases with excellent cycle stability and rate performance were obtained. Solid electrolyte.

Benefits of technology

This method successfully improves the ionic conductivity and cyclic stability of solid electrolytes, significantly enhances the safety and energy density of lithium-ion batteries, extends service life, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009081A_ABST
    Figure CN119009081A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a Li < 6.28 > La < 3 > Zr < 2 > Al < 0.24 > O < 12 > nano solid electrolytic material, which comprises the following steps: uniformly mixing and stirring 80-160 mg of polyacrylic acid, 40-80 mL of water and 160-320 mL of isopropanol, slowly dropwise adding a mixed solution of various salts under a stirring condition, and carrying out ultrasonic reaction for 10 minutes; then adding 500 to 800 [mu] L of ammonia water; washing, freeze-drying, and calcining for 3-5 hours at the temperature of 800-900 DEG C; according to the preparation method disclosed by the invention, the nano-scale Li < 6.28 > La < 3 > Zr < 2 > Al < 0.24 > O < 12 > solid electrolytic material is successfully synthesized by utilizing a template induction and high-temperature calcination technology. Due to the unique nano-size effect, the interface effect of the traditional solid electrolyte can be improved, the ionic conductivity of a sample is effectively enhanced, and excellent cycling stability and rate capability are shown, so that the material is used for the solid electrolyte of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of nanomaterials and their applications, and specifically relates to a nanoscale Li 6.28 La3Zr2Al 0.24 O 12 A method for preparing a solid electrolyte and use of the solid electrolyte as a solid electrolyte for a lithium ion battery. Background Art

[0002] Lithium-ion batteries have the advantages of high energy density, long cycle life and wide operating temperature range. They dominate the energy storage market and bring unprecedented changes to portable electronic devices [Tarascon JM, Armand M. Issues and Challenges Facing Rechargeable Lithium Batteries. Nature, 2001, 414(6861): 359-367; Marques AC, Fuinhas JA, Pereira D A. Have Fossil Fuels Been Substituted by Renewables An Empirical Assessment for 10European Countries. Energy Policy, 2018, 116: 257-265.]. With the rapid development of lithium-ion batteries, the development of smart devices such as smartphones, laptops, and household robots has been promoted, and strong support has been provided for the popularization of electric vehicles. However, existing lithium-ion batteries cannot meet the safety and strict service requirements. Although the electrolyte used in existing batteries has high ion conductivity and excellent electrode surface wettability, it usually has poor thermal stability and electrochemical stability and is regarded as a dangerous product. First, the electrolyte is usually composed of organic solvents, conductive salts and additives, and has strong chemical activity. If the electrolyte leaks, it may react chemically with oxygen or water vapor in the air to produce harmful substances. Secondly, most electrolytes contain flammable organic solvents. If exposed to fire or high temperature environment, they may cause fire or explosion, posing great safety hazards [Nomura Y, Yamamoto K. Advanced Characterization Techniques for Sulfide-Based Solid-State Lithium Batteries. Advanced Energy Materials, 2023, 13(13): 2203883-2203903.]. Lithium-ion batteries urgently need to improve safety, increase energy density, extend cycle life and reduce manufacturing costs [K. Xu. Nonaqueous Liquid Electrolytes for Lithium-Based Rechargeable Batteries. Chemical Reviews, 2004, 104(10): 4303-4417.]. Seeking power batteries with high energy density, low cost and high safety has become an urgent problem to be solved in this field.

[0003] Compared with traditional lithium-ion batteries, all-solid-state lithium-ion batteries are composed of electrode materials and solid electrolytes. They have the advantages of high energy density and high safety performance and are considered to be one of the most promising energy storage devices in the future. On the one hand, solid electrolytes can effectively control the growth of lithium dendrites. At the same time, thanks to the wide electrochemical stability window, excellent thermal stability and strong mechanical strength of solid electrolytes, they show lower volatility and leakage risks compared with liquid electrolytes. These characteristics give solid electrolytes higher energy density, thus having significant advantages over traditional liquid electrolyte systems in terms of safety and performance [Gao Z, Sun H, Fu L, et al. Promises, challenges, and recent progress of inorganic solid-state electrolytes for all-solid-statelithium batteries. Advanced Materials, 2018, 30(17): 1705702.].In particular, garnet-based solid electrolyte materials have attracted extensive attention from scientific researchers due to their high ionic conductivity, good electrochemical stability, high ionic conductivity, very low electronic conductivity, wide electrochemical window and high safety. They are considered to be one of the most promising electrolytes for achieving high energy density and high safety solid-state lithium batteries [JudezX, Eshetu GG, Li C, et al. Opportunities for Rechargeable Solid-StateBatteries Based on Li-Intercalation Cathodes. Joule, 2018, 2(11): 2208-2224;Kravchyk KV, Zhang H, Okur F, et al. Li–Garnet Solid-State Batteries withLLZO Scaffolds. Accounts of Materials Research, 2022, 3(4): 411-415; Tsai CL, Ma Q, Dellen C, et al. A garnet structure-based all-solid-state Li batterywithout interface modification: resolving incompatibility issues on positive electrodes. Sustainable Energy & Fuels, 2019, 3(1): 280-291.]. However, the low grain boundary conductivity and instability of this type of material to lithium limit its development and application. Summary of the invention

[0004] The object of the present invention is to provide a Li 6.28 La3Zr2Al 0.24 O 12 Preparation method of nano solid electrolyte material, garnet-based Li prepared by the method 6.28 La3Zr2Al 0.24 O 12 Solid electrolyte materials have the characteristics of good dispersibility, high cycle stability and long service life.

[0005] Li 6.28 La3Zr2Al 0.24 O 12 A nano solid electrolyte material, which is prepared by the following method, comprising:

[0006] 1) Preparation of a mixed solution of multiple salts: Add 0.600 ~ 1.200 mmol lithium chloride, 0.796 ~ 1.592 mmol lanthanum (III) nitrate hexahydrate, 0.531 ~ 1.062 mmol zirconium chloride and 0.064 ~ 0.128 mmol aluminum chloride to 20 ~ 40 mL water in sequence and stir evenly;

[0007] 2) After 80-160 mg of polyacrylic acid, 40-80 mL of water and 160-320 mL of isopropanol are mixed and stirred evenly, the mixed salt solution obtained in step 1) is slowly added dropwise under stirring, and ultrasonically reacted for 10-30 minutes;

[0008] 3) Under stirring conditions, add 500-800 μL of ammonia water to the mixed solution obtained in step 2), stir and react for 4-5 hours, and centrifuge; repeatedly wash with water and ethanol, and freeze-dry the obtained solid;

[0009] 4) The solid powder obtained in step (3) is calcined at 800-900°C for 3-5 hours in an air atmosphere to obtain Li 6.28 La3Zr2Al 0.24 O 12 Nano solid electrolyte materials;

[0010] The freeze drying in step 2) is performed at -50°C for 36 to 72 hours;

[0011] 40 mL of water described in step 2), 160 mL of isopropanol; 0.600 mmol of lithium chloride described in step 1), 0.796 mmol of lanthanum (III) nitrate hexahydrate, 0.531 mmol of zirconium chloride, 0.064 mmol of aluminum chloride, 20 mL of water; 500 μL of ammonia water described in step 3;

[0012] 80 mL of water described in step 2), 320 mL of isopropanol; 1.200 mmol of lithium chloride described in step 1), 1.592 mmol of lanthanum (III) nitrate hexahydrate, 1.062 mmol of zirconium chloride, 0.128 mmol of aluminum chloride, 40 mL of water; 800 μL of ammonia water described in step 3);

[0013] 80 mL of water described in step 2), 320 mL of isopropanol; 0.800 mmol of lithium chloride described in step 1), 1.061 mmol of lanthanum (III) nitrate hexahydrate, 0.708 mmol of zirconium chloride, 0.085 mmol of aluminum chloride, 30 mL of water; 600 μL of ammonia water described in step 3).

[0014] Another object of the present invention is to provide the Li 6.28 La3Zr2Al 0.24 O 12 Application of nano solid electrolyte materials as solid electrolytes for lithium-ion batteries.

[0015] The present invention provides a Li 6.28 La3Zr2Al 0.24 O 12 The preparation method of nano solid electrolyte material comprises the following steps: 80-160 mg polyacrylic acid, 40-80 mL water and 160-320 mL isopropanol are mixed and stirred evenly, and then the mixed salt solution obtained in step 1) is slowly added dropwise under stirring conditions, and ultrasonically reacted for 10-30 minutes; then 500-800 μL ammonia water is added; washing, freeze drying, and calcining at 800-900°C for 3-5 hours. The present invention utilizes template induction and high temperature calcination technology to successfully synthesize nano-scale Li 6.28 La3Zr2Al 0.24 O 12 Solid electrolyte material. Its unique nano-size effect can improve the interface effect of traditional solid electrolytes, effectively enhance the ionic conductivity of samples, and show excellent cycle stability and rate performance, and is used in solid electrolytes for lithium-ion batteries.

[0016] The present invention has the following advantages:

[0017] 1. Li obtained by the present invention 6.28 La3Zr2Al 0.24 O 12 The solid electrolyte particles are uniform, and their unique nano-size effect improves the interface effect of traditional solid electrolytes and effectively enhances the ionic conductivity of the sample.

[0018] 2. Li prepared by the method of the present invention 6.28 La3Zr2Al 0.24 O 12 Solid electrolyte materials have excellent cycle stability and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The single Li prepared in Example 1 of the present invention 6.28 La3Zr2Al 0.24 O 12 Transmission electron microscope image of nanoparticles;

[0020] Figure 2 Li prepared in Example 1 of the present invention 6.28 La3Zr2Al0.24 O 12 Scanning electron microscope image of nanoparticles;

[0021] Figure 3 Li prepared in Example 1 of the present invention 6.28 La3Zr2Al 0.24 O 12 SEM images of nanoparticle surfaces;

[0022] Figure 4 Li prepared in Example 1 of the present invention 6.28 La3Zr2Al 0.24 O 12 Nanoparticle XRD spectrum;

[0023] Figure 5 Li prepared in Example 1 of the present invention 6.28 La3Zr2Al 0.24 O 12 Cycling performance diagram of material symmetric battery;

[0024] Figure 6 Li prepared in Example 1 of the present invention 6.28 La3Zr2Al 0.24 O 12 Charge and discharge cycle curve of the material;

[0025] Figure 7 Li prepared in Example 1 of the present invention 6.28 La3Zr2Al 0.24 O 12 Rate performance curve of the material. DETAILED DESCRIPTION

[0026] Example 1

[0027] Preparation of Li6.28La3Zr2Al0.24O12 Nano-Solid Electrolyte Materials

[0028] Mix 80 mg of polyacrylic acid, 40 mL of water and 160 mL of isopropanol and stir evenly, then place in a cell crusher. Pipette a mixture of various salts (0.600 mmol of lithium chloride, 0.796 mmol of lanthanum (III) nitrate hexahydrate, 0.531 mmol of zirconium chloride and 0.064 mmol of aluminum chloride dissolved in 20 mL of water) and slowly dropwise add to the above solution, and ultrasonically react for 10 minutes for later use.

[0029] Under stirring conditions, 500 μL of ammonia water was added to the mixed solution and stirred for 4 hours. After the reaction was completed, centrifugation was performed and the sample was repeatedly washed with water and ethanol. The obtained solid was placed in a freeze dryer and heated at -50 °C.o C for 36 hours. o C, calcined at high temperature for 5 hours, obtained Li 6.28 La3Zr2Al 0.24 O 12 Nanomaterials.

[0030] Example 2

[0031] Preparation of Li6.28La3Zr2Al0.24O12 Nano-Solid Electrolyte Materials

[0032] Mix 160 mg of polyacrylic acid, 80 mL of water and 320 mL of isopropanol and stir evenly, then place in a cell crusher. Pipette a mixture of various salts (1.200 mmol of lithium chloride, 1.592 mmol of lanthanum (III) nitrate hexahydrate, 1.062 mmol of zirconium chloride and 0.128 mmol of aluminum chloride dissolved in 40 mL of water) and slowly dropwise add to the above solution, and ultrasonically react for 30 minutes for later use.

[0033] Under stirring conditions, 800 μL of ammonia water was added to the mixed solution and stirred for 5 hours. After the reaction was completed, centrifugation was performed and the sample was repeatedly washed with water and ethanol. The obtained solid was placed in a freeze dryer and heated at -50 °C. o C for 72 hours. o C, calcined at high temperature for 3 hours, Li 6.28 La3Zr2Al 0.24 O 12 Nanomaterials.

[0034] Example 3

[0035] Preparation of Li6.28La3Zr2Al0.24O12 Nano-Solid Electrolyte Materials

[0036] Mix 160 mg of polyacrylic acid, 80 mL of water and 320 mL of isopropanol and stir evenly, then place in a cell crusher. Pipette a mixture of various salts (0.800 mmol of lithium chloride, 1.061 mmol of lanthanum (III) nitrate hexahydrate, 0.708 mmol of zirconium chloride and 0.085 mmol of aluminum chloride dissolved in 30 mL of water) and slowly dropwise add to the above solution, and ultrasonically react for 20 minutes for later use.

[0037] Under stirring conditions, 600 μL of ammonia water was added to the mixed solution and stirred for 3.5 hours. After the reaction was completed, centrifugation was performed and the sample was repeatedly washed with water and ethanol. The obtained solid was placed in a freeze dryer and heated at -50 °C. o C for 56 hours.o C, calcined at high temperature for 5 hours, obtained Li 6.28 La3Zr2Al 0.24 O 12 Nanomaterials.

[0038] Experimental example

[0039] Li prepared in Example 1 6.28 La3Zr2Al 0.24 O 12 Nanoparticles for solid electrolytes in lithium-ion batteries

[0040] 1. Preparation of electrodes: Use lithium iron phosphate as active material, acetylene black as conductive agent, and polyvinylidene fluoride as binder in a certain ratio (active material, conductive agent, polyvinylidene fluoride are 78:10:10) and mix and grind them evenly, then add a small amount of NMP as a dispersant to prepare a uniform slurry. Then, apply the slurry on a 12 mm copper foil and 90 o C was vacuum dried for 12 hours to obtain the positive electrode sheet.

[0041] 2. Preparation of composite solid electrolyte layer: Add 80 mg Li 6.28 La3Zr2Al 0.24 O 12 Powder, 500 mg polyethylene oxide and 170 mg lithium bis(trifluoromethanesulfonyl)imide were mixed and stirred evenly, and then spin-coated into a gel film about 50 μm thick and placed in a vacuum oven for 50 min. o C and dried for 24 h to obtain a composite solid electrolyte layer.

[0042] 3. Assembly of button cells: 2025 type button cells were assembled in a glove box filled with Ar (water and oxygen values ​​were both less than 0.1 ppm), with lithium sheets as counter electrodes and composite solid electrolytes used to match the working electrodes to form button cells.

[0043] 4. Symmetrical battery assembly: 2025 button cells were used in a glove box filled with Ar. Two lithium sheets were placed on both sides of the solid electrolyte membrane for assembly.

[0044] 5. Electrochemical test

[0045] The discharge-charge cycles were performed in the voltage range of 2.0–4.2 V on a battery tester (CT2001A, LAND, China). Cyclic voltammetry (CV) was performed on a CHI760E electrochemical workstation at 0.1 mV s -1The scan rate was between 2.0 and 4.2 V, and the electrochemical impedance spectroscopy (EIS) was obtained on a CHI760E electrochemical workstation with a frequency range of 100 kHz to 0.01 Hz and an amplitude of 5 mV s -1 .

[0046] Long-term stripping / deposition tests show that the solid electrolyte can be stably cycled for 500 hours without short circuit. In addition, the solid-state battery assembled using commercial lithium iron phosphate as the positive electrode and lithium metal as the negative electrode exhibits excellent electrochemical performance at a current density of 0.1 A g -1 , solid-state batteries achieve a stable 170 mAh g -1 And there is no obvious capacity decay after 90 stable cycles. The rate performance test further proves the high electrochemical stability of the solid-state battery.

Claims

1. Li 6.28 La3Zr2Al 0.24 O 12 A nano solid electrolyte material, which is prepared by the following method, comprising: 1) Preparation of a mixed solution of multiple salts: Add 0.600 ~ 1.200 mmol lithium chloride, 0.796 ~ 1.592 mmol lanthanum (III) nitrate hexahydrate, 0.531 ~ 1.062 mmol zirconium chloride and 0.064 ~ 0.128 mmol aluminum chloride to 20 ~ 40 mL water in sequence and stir evenly; 2) After 80-160 mg of polyacrylic acid, 40-80 mL of water and 160-320 mL of isopropanol are mixed and stirred evenly, the mixed salt solution obtained in step 1) is slowly added dropwise under stirring, and ultrasonically reacted for 10-30 minutes; 3) Under stirring conditions, add 500-800 μL of aqueous ammonia to the mixed solution obtained in step 2), stir and react for 4-5 hours, and centrifuge; The solid was washed repeatedly with water and ethanol and freeze-dried; 4) The solid powder obtained in step (3) is calcined at 800-900°C for 3-5 hours in an air atmosphere to obtain Li 6.28 La3Zr2Al 0.24 O 12 Nano solid electrolyte materials.

2. Li according to claim 1 6.28 La3Zr2Al 0.24 O 12 Nano solid electrolyte material, characterized by: The freeze drying in step 2) is performed at -50°C for 36 to 72 hours.

3. Li according to claim 1 or 2 6.28 La3Zr2Al 0.24 O 12 Nano solid electrolyte material, characterized by: 40 mL of water described in step 2), 160 mL of isopropanol; 0.600 mmol of lithium chloride described in step 1), lanthanum (III) nitrate hexahydrate 0.796 mmol, zirconium chloride 0.531 mmol, aluminum chloride 0.064 mmol, water 20 mL; ammonia water 500 μL described in step 3).

4. Li according to claim 1 or 2 6.28 La3Zr2Al 0.24 O 12 Nano solid electrolyte material, characterized by: 80 mL of water described in step 2), 320 mL of isopropanol; 1.200 mmol of lithium chloride described in step 1), lanthanum (III) nitrate hexahydrate 1.592mmol, zirconium chloride 1.062mmol, aluminum chloride 0.128mmol, water 40mL; ammonia water 800μL described in step 3).

5. Li according to claim 1 or 2 6.28 La3Zr2Al 0.24 O 12 Nano solid electrolyte material, characterized by: 80 mL of water described in step 2), 320 mL of isopropanol; 0.800 mmol of lithium chloride described in step 1), lanthanum (III) nitrate hexahydrate 1.061mmol, zirconium chloride 0.708mmol, aluminum chloride 0.085mmol, water 30mL; ammonia water 600μL described in step 3).

6. Li according to claim 6.28 La3Zr2Al 0.24 O 12 Application of nano solid electrolyte materials as solid electrolytes for lithium-ion batteries.