Sodium ion sulfide solid electrolyte and preparation method thereof

By introducing molybdenum and oxygen doping into the sodium ion sulfide solid electrolyte, the chemical composition of Na3-xSb1-xWxS4-yOy is solved, and the problem of taking into account the high ionic conductivity and cyclic stability properties of sodium ion sulfide solid electrolyte is solved. , realizes efficient ion conduction and interface stability, and meets the development needs of all-solid-state batteries.

CN119009086AInactive Publication Date: 2024-11-22NINGBO UNIV

Patent Information

Application Number
CN202411475802.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-22
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing sodium ion sulfide solid electrolytes are difficult to take into account between high ionic conductivity and cyclic stability performance. In particular, Na3SbS4 is prone to redox reactions when contacting Na metal anode, resulting in interface instability, reducing battery capacity and cycle life.

Method used

By introducing molybdenum (W) and oxygen (O) doping, the chemical composition of Na3-xSb1-xWxS4-yOy is formed, using high concentration W to compensate for charge in the lattice and form cubic phases, increasing Na vacancy to achieve three-dimensional ion conduction, The Na metal anode is protected by introducing a self-passivation layer through O to improve interface stability.

Benefits of technology

It achieves high ionic conductivity (order 10-2) and significantly improves cycle stability performance, extends the stabilization time between the electrolyte and the metal anode interface, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009086A_ABST
    Figure CN119009086A_ABST
Patent Text Reader

Abstract

The invention discloses a sodium ion sulfide solid electrolyte and a preparation method thereof, the chemical composition formula of the sodium ion sulfide solid electrolyte is Na < 3-x > Sb < 1-x > W < x > S < 4-y > O < y >, and x and y are respectively the molar ratio 0 < lt > of an element W and an element O in the sodium ion sulfide solid electrolyte; x is greater than or equal to 0 and less than or equal to 0.4, y is greater than or equal to 0 and less than or equal to 0.3, a crystal phase of the sodium ion sulfide solid electrolyte is c-Na3SbS4, and a unit cell center is composed of SbS43 and WS42. W and O are introduced at a high concentration, Na vacancies can be effectively generated in a crystal lattice in the Na3SbS4 crystal through charge compensation, distortion in the C-axis direction is reduced, formation of a cubic phase is facilitated, isotropic 3D fast ion conduction is promoted, and high ion conductivity of 10 <-2 > orders of magnitude can be achieved; and meanwhile, a self-passivation layer can be generated at the interface of the electrolyte and the Na metal anode, so that the cycling stability of the electrolyte is fundamentally improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid electrolytes and preparation thereof, and specifically relates to a sodium ion sulfide solid electrolyte and a preparation method thereof. Background Art

[0002] The combustion and leakage of organic liquid electrolytes is a long-standing challenge in battery safety. All-solid-state sodium-ion batteries have the advantages of being non-volatile and non-flammable, which can effectively solve these safety hazards. There are two common substrates for solid electrolytes, namely oxide substrates and sulfide substrates. The most important advantage of oxide-based solid electrolytes is that they are more stable in air at room temperature and at high temperatures, while their biggest disadvantage is that it is difficult to achieve an ionic conductivity of 10 -3 In contrast, the properties of sulfide-based solid electrolytes are completely opposite to those of oxide-based solid electrolytes. 2- The electronegativity of O 2- The small size reduces the attraction to sodium ions, which helps to form a suitable sodium ion transmission channel. Therefore, sulfide-based solid electrolytes can usually achieve higher ion conductivity, but their stability is relatively low. Therefore, how to make up for the disadvantages of sulfide-based solid electrolytes while ensuring their advantages is widely considered to be one of the technical problems that urgently need to be overcome.

[0003] At present, the research on Na3SbS4 solid electrolytes often focuses on how to obtain higher ionic conductivity, while ignoring the interfacial instability caused by the redox reaction of Na3SbS4 solid electrolytes in contact with Na metal anodes. Over time, this interfacial instability will reduce the capacity and cycle life of the battery. In addition to ionic conductivity, achieving long-term stable and safe electroplating / stripping is also a key performance that batteries with potential commercial application value need to have. Therefore, the research on sodium ion sulfide solid electrolytes with high ionic conductivity, especially the research on solid electrolytes with good cycle stability, is highly anticipated. In view of this, the present invention proposes a sodium ion sulfide solid electrolyte and a preparation method thereof. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a sodium ion sulfide solid electrolyte having both high ionic conductivity and cyclic stability and a preparation method thereof in view of the deficiencies in the prior art.

[0005] The technical solution adopted by the present invention to solve the above technical problems is: a sodium ion sulfide solid electrolyte, the chemical composition formula of which is Na 3-x Sb 1-x W x S 4-y O y, where x and y are the molar ratios of element W and element O in the sodium sulfide solid electrolyte respectively, 0 < x ≤ 0.4, 0 ≤ y ≤ 0.3, the crystal phase of the sodium sulfide solid electrolyte is c-Na3SbS4, and the center of the unit cell of the sodium sulfide solid electrolyte consists of SbS4 3− and WS4 2− .

[0006] Preferably, the molar ratio of element W in the sodium sulfide solid electrolyte is 0.2 ≤ x ≤ 0.4. This high-concentration W doping can ensure the high ionic conductivity of the sodium sulfide solid electrolyte.

[0007] The preparation method of the above sodium sulfide solid electrolyte includes the following steps: (1) Weigh the raw materials Na2S, Sb2S3, WS2, WO3, and S in different proportions inside a glove box filled with argon, control the error within ±0.001 g, put the above raw materials into the ball milling tank of a ball mill for mixed ball milling treatment, and then take out the mixed sample from the ball milling tank inside the glove box to obtain the precursor of the sample; (2) Press the precursor into a block, put it into a quartz tube, evacuate the quartz tube to 10 -4 Pa, and then encapsulate the precursor in the quartz tube; (3) Put the encapsulated quartz tube into an annealing furnace, first heat it at a heating rate of 5 °C / min to 580 - 620 °C, then anneal it at 580 - 620 °C for 12 h, and then cool it to room temperature at a cooling rate of 1 - 5 °C / min. Open the quartz tube to obtain the sodium sulfide solid electrolyte.

[0008] Preferably, in step (1), the condition parameters inside the glove box are: the moisture content is less than 1 ppm and the oxygen content is less than 1 ppm.

[0009] Preferably, in step (1), the conditions for the mixed ball milling treatment are: the rotation speed is 500 rpm, the ball-to-material ratio is 20:1, the ball milling time is 20 h. During the mixed ball milling treatment, a counterclockwise rotation mode is adopted, the cycle is set to ball mill for 15 min and pause for 5 min, and during the ball milling period, scraping is carried out every 5 - 10 h.

[0010] Preferably, in step (2), the pressure used to press the precursor into a block is 240 - 300 MPa.

[0011] Compared with the prior art, the present invention has the following advantages: 1) The sodium ion sulfide solid electrolyte of the present invention introduces W at a high concentration, which can effectively generate Na vacancies in the lattice through charge compensation in the Na3SbS4 crystal, and reduce the distortion in the C-axis direction, which is conducive to the formation of the cubic phase; Different from the light doping, the present invention introduces high concentration W, and after a large number of vacancies participate, the ion movement in the lattice can realize three-dimensional transmission, and Na ions can jump into adjacent vacancies and then be transmitted, thereby promoting isotropic 3D fast ion conduction, which can reach 10 -2 Orders of magnitude higher ionic conductivity; 2) The sodium ion sulfide solid electrolyte of the present invention is doped with W and O is introduced, so that when the electrolyte is applied to a sodium ion battery, a self-passivation layer can be generated at the interface between the electrolyte and the Na metal anode, thereby protecting the Na metal anode, limiting the reduction of the interface, stabilizing the interface between the electrolyte and the metal anode, and fundamentally improving the cycle stability of the electrolyte; 3) The preparation method of the sodium ion sulfide solid electrolyte of the present invention obtains a precursor by mixing and ball milling the mixed raw materials, and then heats the precursor in a vacuum environment, which can make the reaction more complete, effectively eliminate the grain boundary impedance of the electrolyte, and improve the ionic conductivity. This method can simply and quickly obtain a bulk electrolyte with uniform composition and good comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 XRD patterns of the electrolyte sample powders of Examples 1 to 4; Figure 2 The Raman spectra of the electrolyte sample powders of Examples 1 to 4; Figure 3 XRD patterns of the electrolyte sample powders of Examples 3 and 5-7; Figure 4 The Raman spectra of the electrolyte sample powders of Examples 3 and 5-7; Figure 5 The Nyquist impedance spectra of the electrolyte sample powders of Examples 1 to 7 and the comparative example; Figure 6 The calculated results of ionic conductivity of the electrolyte samples of Examples 1 to 7 and the comparative example; Figure 7 is a unit cell diagram of the electrolyte sample powder of Example 1; Figure 8 is a unit cell diagram of the electrolyte sample powder of Example 3; Fig. 9 The electrolyte sample of Example 6 23 Na NMR fitting line; Fig.10 is the critical current density of the electrolyte sample of Example 3; Fig.11 is the critical current density of the electrolyte sample of Example 6; Fig.12 The electrolyte samples of Examples 3 and 6 were at 0.1 mA / cm 2 Stable plating / stripping curves under . DETAILED DESCRIPTION

[0013] The present invention is further described in detail below with reference to the accompanying drawings, embodiments and comparative examples.

[0014] The present invention provides a total of 7 embodiments and 1 comparative example of sodium ion sulfide solid electrolytes. The molar ratio of element W and element O in each electrolyte, the chemical composition formula, and the amount of raw materials are shown in Table 1. 5 g of each electrolyte sample of Embodiment 1 to Embodiment 7 and the comparative example are prepared respectively.

[0015] The preparation method of the sodium ion sulfide solid electrolyte of Example 1 to Example 7 is: (1) In a glove box filled with argon gas, with a moisture content of less than 1 ppm and an oxygen content of less than 1 ppm, the raw materials Na2S (purity 95%), Sb2S3 (purity 99%), WS2 (purity 99.9%), WO3 (purity 99.9%) and S (purity 99.99%) were weighed in different proportions, with the error controlled within ±0.001 g. The raw materials were placed in a ball mill for mixed ball milling. The mixed ball milling conditions were: a rotation speed of 500 rpm, a ball-to-material ratio of 20:1, and a ball milling time of 20 h. During the mixed ball milling process, a counterclockwise rotation mode was adopted. The cycle was set to ball milling for 15 min and pause for 5 min. During the ball milling process, the scraping process was performed every 10 h. After the mixed ball milling process, the mixed sample was taken out from the ball mill in the glove box to obtain a precursor of the sample. (2) Press the precursor into a block at a pressure of 240 MPa, place it in a quartz tube, and evacuate the tube to 10 -4 After Pa, the precursor is encapsulated in a quartz tube; (3) The packaged quartz tube was placed in an annealing furnace, first heated to 600°C at a heating rate of 5°C / min, then annealed at 600°C for 12 h, and then cooled to room temperature at a cooling rate of 1°C / min. The quartz tube was opened to obtain a cylindrical bulk sample of the sodium ion sulfide solid electrolyte with a diameter of 10 mm and a thickness of about 0.5 mm.

[0016] The preparation method of the sodium ion sulfide solid electrolyte of the comparative example is the same as that of Examples 1 to 7, the only difference being the ratio of raw materials.

[0017] Phase analysis and electrochemical analysis were performed on the electrolyte samples of Examples 1 to 7 and the comparative example, respectively, and the specific steps were as follows: The electrolyte samples of Examples 1 to 7 and the comparative example were processed into powders, and 100 mg of the sample powders were weighed and placed in a polyimide container for phase analysis. Examples 1 to 4 were subjected to XRD analysis at room temperature (25°C). The XRD patterns are shown in Figure 1 ( Figure 1 c-Na3SbS4 and t-Na3SbS4 represent standard cards respectively), Raman spectrum see Figure 2 .from Figure 1 It can be seen that in Example 3, the double peaks merged into a single peak, which means that the tetragonal distortion of the lattice is reduced, resulting in the crystal phase changing to a cubic phase. Figure 2 It can be seen that under different W contents, the Raman peak position does not change significantly, but the relative intensity changes, confirming the doping effect. Based on Example 3, O is introduced into Examples 5 to 7, and the molar ratio of WO3 increases successively. The XRD spectra of the electrolyte sample powders of Examples 3 and 5 to 7 are shown in Figure 3 ( Figure 3 c-Na3SbS4 and Na2WO4 represent standard cards respectively), Raman spectrum see Figure 4 .from Figure 3 The effect of introducing O on the electrolyte can be seen. After the introduction of O, the XRD diffraction peaks of the electrolyte are narrow and sharp, indicating that the electrolyte introduced with O has good crystallinity. Although a small amount of NaSbS2 impurities are observed from these peaks, the sample is mainly composed of cubic phase NSS. Therefore, regulating the amount of O introduced can achieve the regulation of other aspects of the electrolyte performance on the basis of maintaining the original conductive structure of the electrolyte.

[0018] On an electrochemical workstation, the electrochemical properties of the electrolyte sample powders of Examples 1 to 7 and the comparative example were studied using AC complex impedance. The Nyquist impedance spectra of the electrolyte sample powders of Examples 1 to 7 and the comparative example are shown in Figure 5 .from Figure 5 It can be seen that the impedance of the electrolyte sample powder of Example 3 is as low as 1.8Ω. After increasing the O content, the ionic conductivity of the electrolyte sample powder of Example 6 still retains 10 -2 The test method of ionic conductivity is as follows: 100 mg of electrolyte sample powder is weighed and placed in an impedance mold with a diameter of 10 mm, and a pressure of 240 MPa is applied to press it into a sheet, and the AC impedance of the electrolyte is tested at room temperature, the disturbance voltage is 10 mV, and the test range is 1 MHz~1 Hz. Figure 6 Calculation results of ionic conductivity of electrolyte samples of Examples 1 to 7 and Comparative Examples. Figure 6It can be seen that the electrolyte samples of Examples 1 to 7 all have high ionic conductivity, and most of them can reach 10 -2 The ionic conductivity of the electrolyte sample of Example 3 is the highest, which is 3.513×10 -2 S / cm, followed by the electrolyte sample of Example 2 at 2.9×10 -2 S / cm.

[0019] The space group of the electrolyte sample powder of Example 1 is , the unit cell parameters are: a=b=7.161413Å, c=7.273668Å, V=373.036156 Å 3 Its crystal structure is determined to be tetragonal, that is, the center of the unit cell is SbS4 3− and WS4 2− The XRD data of the electrolyte sample powder of Example 1 was refined to obtain the lattice parameters and draw a unit cell diagram, as shown in FIG. Figure 7 shown.

[0020] The space group of the electrolyte sample powder of Example 3 is , the unit cell parameters are: a=b=c=7.196108Å, V=372.643022Å 3 Its crystal structure is determined to be cubic, with the center of the unit cell being SbS4 3− and WS4 2− The XRD data of the electrolyte sample powder of Example 3 was refined to obtain the lattice parameters and draw a unit cell diagram, as shown in FIG. Figure 8 shown.

[0021] Fig. 9 The electrolyte sample of Example 6 23 The Na NMR fitting line shows that the fitting line is nearly identical to the experimental line of Example 6 due to the good fitting degree. By fitting the Gaussian and Lorentzian components, several peaks due to the influence of Na at different sites can be observed. By identifying the changes in the peak area, the transmission path of the sodium ions can be reflected. The new resonance peak at 17 ppm (i.e. Fig. 9 Peak 1 in the figure proves that the Na vacancies brought by the introduction of W are beneficial to the transport of Na ions in the lattice.

[0022] In order to detect the cycle stability performance of the electrolyte samples, for the electrolyte samples of Example 3 and Example 6, the electrolyte sample powders of Example 3 and Example 6 were respectively pressed into small discs with a diameter of 10 mm using a portable battery testing instrument LAND CT2001 at a pressure of 240 MPa, and symmetrical batteries were prepared using metal Na sheets as electrodes. The battery long cycle and critical current density tests were performed at 25°C. Fig.10 and Fig.11 They are the critical current densities of the electrolyte samples of Example 3 and Example 6 respectively. Fig.10 and Fig.11 It can be seen that the critical current density of the electrolyte sample of Example 6 is greater than that of Example 3.

[0023] For the electrolyte samples of Example 3 and Example 6, a DC cycle test was performed under the same conditions, wherein the current density used in the DC cycle test was 0.1 mA / cm -2 , the test results are as follows Fig.12 As shown. Fig.12 It can be seen that compared with the electrolyte sample of Example 3, the stable cycle time of the electrolyte sample of Example 6 increased by 4.5 times, and it has better cycle stability performance. The ionic conductivity of the electrolyte sample of Example 6 is 1.774×10 -2 S / cm.

[0024] In summary, by controlling the chemical composition of the sodium ion sulfide solid electrolyte of the present invention and regulating the introduction amount of element W and element O, the comprehensive performance of the electrolyte can be regulated, the ionic conductivity and cycle stability of the electrolyte can be improved and taken into account, and the development needs of all-solid-state batteries can be met.

[0025]

Claims

1. A sodium ion sulfide solid electrolyte, It is characterized in that The chemical composition formula of the sodium-ion sulfide solid electrolyte is Na 3-x Sb 1-x W x S 4-y O y , where x and y are the molar ratios of element W and element O in the sodium-ion sulfide solid electrolyte respectively, 0 < x ≤ 0.4, 0 ≤ y ≤ 0.3, and the crystal phase of the sodium-ion sulfide solid electrolyte is c-Na 3 SbS 4 , the center of the unit cell of the sodium-ion sulfide solid electrolyte is composed of SbS 4 3− and WS 4 2− .

2. A sodium ion sulfide solid electrolyte according to claim 1, It is characterized in that 0.2≤x≤0.4。 3. A method for preparing the sodium ion sulfide solid electrolyte according to claim 1 or 2, It is characterized in that The following steps are involved: (1) In a glove box filled with argon, weigh the raw materials Na and 2 S, Sb 2 S 3 , WS 2 , WO 3 and S, with the error controlled within ±0.001 g, the above raw materials are placed in a ball milling jar of a ball mill for mixed ball milling, and then the mixed sample is taken out from the ball milling jar in a glove box to obtain a precursor of the sample; (2) Press the precursor into a block, place it in a quartz tube, and evacuate the tube to 10 -4 After Pa, the precursor is encapsulated in a quartz tube; (3) placing the packaged quartz tube into an annealing furnace, first heating the temperature to 580-620°C at a heating rate of 5°C / min, then annealing at 580-620°C for 12 h, and then cooling the tube to room temperature at a cooling rate of 1-5°C / min. The quartz tube is opened to obtain the sodium ion sulfide solid electrolyte.

4. The method for preparing the sodium ion sulfide solid electrolyte according to claim 3, It is characterized in that In step (1), the condition parameters in the glove box are: the moisture content is less than 1 ppm, and the oxygen content is less than 1 ppm.

5. The method for preparing the sodium ion sulfide solid electrolyte according to claim 3, It is characterized in that In step (1), the conditions for the mixed ball milling treatment are: rotation speed 500 rpm, ball-to-material ratio 20:1, ball milling time 20 h. During the mixed ball milling treatment, a counterclockwise rotation mode is adopted, and the cycle is set to ball milling for 15 min and pause for 5 min. During the ball milling, the scraping treatment is performed every 5 to 10 h.

6. The method for preparing the sodium ion sulfide solid electrolyte according to claim 3, It is characterized in that In step (2), the pressure used to press the precursor into blocks is 240~300MPa.

Citation Information

Patent Citations

  • Air-stable sulfide sodium ion solid electrolyte and preparation method thereof

    CN108390094A

  • Solid electrolyte for all-solid-state sodium battery, manufacturing method therefor, and all-solid-state sodium battery

    CN112470317A

  • High-ionic-conductivity sulfide solid electrolyte membrane and preparation method and application thereof

    CN118136932A

  • Method for producing metal-and / or semimetal-containing sulfide, and sodium-containing sulfide

    CN118302380A

  • Electrode active material-solid electrolyte composite, method for manufacturing the same, and all solid state rechargeable lithium battery including the same

    KR1020180033838A

Cited By

  • Inflammable sodium battery and preparation method thereof

    CN119944044A

  • Battery monomer, preparation method thereof, battery device and power utilization device

    CN122202481A