Composite polymer solid electrolyte integrated by trace amphoteric molecular filler and preparation method and application of composite polymer solid electrolyte
By using composite polymer solid electrolyte integrated with trace amphoteric molecular-grade fillers in lithium metal solid-state batteries, the problem of insufficient mechanical strength and stability of the electrolyte of lithium metal solid-state batteries is solved, and efficient lithium ion transmission and battery cycle stability is achieved. .
Patent Information
- Application Number
- CN202411429287.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-22
AI Technical Summary
The solid electrolytes of existing lithium metal solid-state batteries have shortcomings in terms of mechanical strength, refraction resistance and electrochemical stability, and the interface between the filler and the polymer is prone to deterioration during long-term use, affecting the lithium ion transmission performance.
Using a composite polymer solid electrolyte integrated with trace amphoteric molecular-grade filler, a composite polymer film is prepared by dispersing lithium salts and amphoteric molecular-grade fillers in an organic polymer matrix to form an efficient lithium ion conductive path, and a composite polymer film is prepared under vacuum. Ensure compatibility between the electrolyte and the electrode.
It significantly improves the conductivity and mechanical properties of lithium ion, extends the cycling stability of lithium metal symmetrical batteries, inhibits the growth of lithium protrusions and dendrites, and achieves high capacity release and good conversion reaction reversibility.
Smart Images

Figure CN119009106A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy technology, and in particular to a composite polymer solid electrolyte integrated with trace amphiphilic molecular-level fillers, and a preparation method and application thereof. Background Art
[0002] Lithium metal solid-state batteries are considered to be one of the most promising electrochemical energy storage systems due to their significant improvement in energy density compared to existing lithium-ion batteries. Inorganic solid electrolytes based on representative materials such as oxides, sulfides, and halides exhibit a high energy density of about 10 -4 Up to 10 -2 S cm -1 Solid electrolytes have ideal ionic conductivity, but their brittleness and poor mechanical properties lead to high interfacial contact resistance. In contrast, solid electrolytes based on polymer matrices are more suitable for commercial applications due to their excellent mechanical flexibility, interfacial compatibility, easy preparation and cost-effectiveness. Polyethylene oxide (PEO) is a commonly used polymer matrix in solid polymer electrolytes and is favored for its excellent operability and efficient lithium salt dissociation ability. However, ionic conduction in PEO electrolytes mainly occurs in the amorphous part of the PEO matrix, while the crystalline part contributes very little to ion movement. Therefore, the ionic conductivity of PEO electrolytes depends largely on the ability of the polymer matrix to dissolve lithium salts and the ratio of the crystalline phase to the amorphous phase. To this end, modification strategies are widely used to improve the ionic conductivity of PEO electrolytes.
[0003] Plasticizers are added to PEO to improve its ionic conductivity. However, this strategy leads to decreased mechanical strength, fire resistance, and electrochemical stability of solid polymer electrolytes. Direct synthesis of PEO into polymer networks, such as comb or star structures, can significantly reduce the crystallization of PEO. However, most of the current synthesis processes have the problems of cumbersome operations or harsh reaction conditions. Adding ion conductive fillers such as Li7La3Zr2O to PEO 12 (LLZO) and Li 1.3 Al 0.3 Ti 1.7 (PO4)3(LATP) is another effective approach. Although these conductive fillers provide sufficient lithium ion conductivity in the composite structure, the interface between the heavy metal-containing ceramic material and the polymer in the composite electrolyte may degrade over time due to potential side reactions or gravity separation. This degradation not only weakens the mechanical strength, but also affects the Li+ transfer performance of the solid polymer electrolyte during long-term cycling. + Transmission performance is negatively affected.
[0004] Recently, functional fillers have been highly anticipated due to their multiple enhancement effects. They are usually based on two-dimensional (2D) materials or metal-organic frameworks (MOFs) and have attractive properties such as high ionic conductivity, mechanical strength, effective electrolyte interface contact, and enhanced stability. However, compared with inorganic ceramic electrolytes, these functional filler / polymer composite electrolytes require more complicated preparation processes to effectively fuse fillers and polymers. More importantly, the filler content is relatively large, usually exceeding 10 wt%, which may not form a uniform fast Li+ / Li+ bond between the filler and the polymer. + transmission channel, but only plays a role in the fast Li + In addition, the fluoride conversion cathode paired with a lithium metal anode can theoretically provide up to 712 mAh g -1 Unfortunately, it is often affected by the failure and dissolution of conversion products, resulting in fluorine loss and rapid capacity decay, which is particularly evident during the early cycles. Summary of the invention
[0005] The first technical problem to be solved by the present invention is: in view of the deficiencies in the prior art, a composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers is provided, which has good conductivity and strong compatibility with electrodes.
[0006] To solve the above-mentioned first technical problem, the technical solution of the present invention is:
[0007] A composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers comprises an organic polymer matrix, and lithium salt and amphiphilic molecular fillers dispersed in the organic polymer matrix.
[0008] Preferably, the organic polymer includes at least one of polyethylene oxide, polyacrylonitrile, polyethylene glycol, polyvinylidene fluoride, and poly(vinylidene fluoride-co-hexafluoropropylene);
[0009] The lithium salt includes at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium hexafluorophosphate, and lithium perchlorate.
[0010] Preferably, the mass fraction of the amphoteric molecular filler in the composite polymer solid electrolyte is 0.5wt% to 10wt%.
[0011] Preferably, the amphiphilic molecular grade filler includes at least one of amino acids such as cysteine, glutamic acid, lysine, and asparagine.
[0012] Preferably, the molar mass of the organic polymer is calculated based on the molar mass of the polymerized monomer used to form the organic polymer, and the molar ratio of the organic polymer monomer to the lithium salt is (10-20):1.
[0013] Preferably, the organic polymer monomer is a polyethylene oxide monomer, wherein the polyethylene oxide monomer: lithium salt = ethylene oxide C2H4O monomer: lithium salt = (10-20):1.
[0014] Preferably, the thickness of the composite solid electrolyte integrated with trace amphiphilic molecular-level fillers is 18 to 100 μm.
[0015] Using amphiphilic small molecule particles as filler raw materials for polymer electrolytes, a composite solid electrolyte membrane integrated with trace amphiphilic molecular-level fillers was prepared. Among them, the amphiphilic small molecule particles are dissolved in the polymer system and no longer retain the particle structure, realizing a fully homogeneous polymer electrolyte system. Due to the strong interaction between trace amphiphilic small molecules and polymers and lithium salts, the conductivity of the composite polymer electrolyte is greatly improved. Trace amphiphilic molecular-level fillers can also promote the dissociation of lithium salts in the polymer system and increase the lithium ion migration number of the polymer electrolyte. The addition of trace amphiphilic molecular-level fillers quickly forms a chemically stable SEI film derived from lithium salts and organic polymers, and the lamellar uniform deposition of lithium mechanically inhibits the growth of lithium protrusions and dendrites. Based on the good compatibility of the composite polymer electrolyte with the electrode, it is ensured that even in the configuration of a thin electrolyte membrane, the Li-Fe-F conversion solid-state battery can achieve high capacity release and better reversibility of the conversion reaction.
[0016] The second technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a method for preparing a composite polymer solid electrolyte integrated with trace amphiphilic molecular-level fillers is provided, and the prepared composite polymer solid electrolyte has good electrical conductivity and strong compatibility with electrodes.
[0017] To solve the above second technical problem, the technical solution of the present invention is:
[0018] A method for preparing a composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers comprises the following steps:
[0019] S1, adding an organic polymer, a lithium salt and amphiphilic molecular filler particles into an organic solvent, and mixing to obtain a mixed slurry;
[0020] S2, pouring the obtained mixed slurry on a substrate to form a composite polymer film precursor;
[0021] S3. Heat the substrate coated with the composite polymer film precursor to 40-80° C. under vacuum conditions, keep it warm for at least 24 hours, and then air-cool it to room temperature to obtain the composite polymer solid electrolyte integrated with the trace amphiphilic molecular-level filler.
[0022] Preferably, the organic solvent is one of acetonitrile, dimethylformamide and N-methylpyrrolidone;
[0023] The mixing method is stirring, and the stirring is stirring at room temperature to 60° C. for 4 to 8 hours.
[0024] Preferably, the substrate is a polytetrafluoroethylene plastic plate.
[0025] The organic polymer, lithium salt and organic amphiphilic molecular filler particles are mixed and dissolved in an organic solvent, and then dried in a polytetrafluoroethylene mold to obtain a composite polymer solid electrolyte membrane. The amphiphilic molecular filler particles interact with the organic polymer and lithium salt to ensure the precise control of the mechanical properties and thickness of the final polymer solid electrolyte membrane integrated with trace amphiphilic molecular fillers.
[0026] The third technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a lithium metal symmetric battery system based on a composite polymer solid electrolyte is provided, and the battery has good cycle stability.
[0027] To solve the third technical problem, the technical solution of the present invention is:
[0028] A lithium metal symmetric battery system based on a composite polymer solid electrolyte, the lithium metal symmetric battery system comprising a composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers, and metal lithium sheets located on both sides of the composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers.
[0029] When the composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers is used in lithium metal symmetric batteries, it has good interface stability and extremely low interface impedance, can significantly reduce the voltage polarization difference during the deposition / stripping process of metal lithium, enhance the cycle stability of the symmetric battery, and the metal lithium surface of the symmetric battery remains smooth and dense after long-term cycling.
[0030] The fourth technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a solid-state lithium metal battery based on a composite polymer solid electrolyte is provided, and the battery has good cycle stability.
[0031] To solve the fourth technical problem, the technical solution of the present invention is:
[0032] A solid-state lithium metal battery based on a composite polymer solid electrolyte comprises a positive electrode, a negative electrode, and a composite polymer solid electrolyte integrated with a trace amount of amphiphilic molecular filler located between the positive electrode and the negative electrode.
[0033] Preferably, the negative electrode is a metal lithium sheet, and the positive electrode is at least one of ferric trifluoride, ferrous fluoride, iron oxyfluoride, copper fluoride, copper hydroxide fluoride, carbon-sulfur composite, ferrous disulfide, lithium manganate, lithium iron phosphate, lithium cobalt oxide, nickel-rich ternary system and lithium-rich manganese-based solid solution.
[0034] The fifth technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a solid-state lithium / fluoride battery with a soft-pack configuration based on a composite polymer solid electrolyte is provided, and the battery has good cycle stability.
[0035] To solve the fifth technical problem, the technical solution of the present invention is:
[0036] A solid lithium / fluoride battery with a soft-pack configuration based on a composite polymer solid electrolyte, the soft-pack battery comprising a positive electrode, a negative electrode, and a composite polymer solid electrolyte integrated with a trace amount of amphiphilic molecular filler located between the positive electrode and the negative electrode.
[0037] Preferably, the negative electrode is a thin-layer metallic lithium, and the positive electrode is at least one of ferric fluoride, ferrous fluoride, iron oxyfluoride, copper fluoride, and copper hydroxide fluoride.
[0038] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0039] 1. The present invention uses trace amphiphilic molecular fillers to prepare a composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers. This trace amphiphilic molecular filler is linked with the polymer matrix through physical entanglement and hydrogen bonds, which effectively ensures the mechanical performance advantages of the electrolyte membrane during the thinning process, and realizes the manufacture of ultra-thin composite polymer membranes with a minimum thickness of 18μm.
[0040] 2. Trace amount of amphiphilic filler and TFSI in the present invention - The anionic interaction promotes the dissociation of lithium salts, thus achieving fast Li + The lithium ion transfer number reaches 0.68. In addition, the rich functional groups contained in the trace amphiphilic molecular fillers promote the in-situ formation of a stable solid electrolyte interface (SEI) protective layer at the electrolyte / electrode interface, which synergistically enhances the cycle stability of the symmetric battery.
[0041] 3. The trace amphiphilic molecular fillers in the present invention also give lithium iron fluoride conversion batteries excellent rate performance and long-term cycle stability. These batteries can still maintain a high capacity after 700 cycles at a rate of 0.5C. In addition, the fluorine-based solid-state soft-pack battery was successfully operated, effectively promoting the future practical application of fluorine-based battery systems. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 Optical photograph of a composite polymer solid electrolyte integrated with trace amounts of amphiphilic molecular fillers;
[0043] Figure 2 The morphology of the composite polymer solid electrolyte integrated with trace amphiphilic fillers;
[0044] Figure 3 The ionic conductivity diagram of the composite polymer solid electrolyte at 30℃ and 60℃ with different cysteine (LCy) contents;
[0045] Figure 4 A Li||Li symmetric cell with a trace amount of amphiphilic fillers integrated into a composite polymer solid electrolyte and pure polymer electrolyte at 0.2 mA cm -2 Constant current cycle performance and amplified voltage curve under ;
[0046] Figure 5 SEM image of the lithium metal deposition surface of a lithium metal symmetric battery with a composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers after 120 hours of cycling;
[0047] Figure 6 Cycling performance diagram of solid-state Li||FeF3 battery with composite polymer solid electrolyte integrated with trace amphiphilic fillers at 0.5C rate and voltage range of 1.2-3.9V;
[0048] Figure 7 The charge and discharge curves of the solid-state Li||FeF3 battery with a composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers at different electrochemical cycle stages at a rate of 0.5C and a voltage range of 1.2-3.9V;
[0049] Figure 8 Optical photograph of solid-state Li||FeF3 soft-pack battery with composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers;
[0050] Fig. 9 Cycling performance diagram of solid-state Li||FeF3 soft-pack battery with composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers;
[0051] Fig.10 Abuse experiment of solid-state Li||FeF3 soft-pack battery with composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers;
[0052] Fig.11 The cycling performance diagram of solid-state Li||FeF3 battery with pure PEO polymer solid electrolyte at 0.2C rate and voltage range of 1.2-3.9V. DETAILED DESCRIPTION
[0053] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.
[0054] The present invention uses trace amphiphilic molecules as fillers of polymer electrolytes to prepare composite solid electrolytes integrated with trace amphiphilic molecular fillers. Among them, due to the simple molecular structure of the amphiphilic molecular filler particles and their rich functional groups (carboxyl, amino and thiol), lithium ion transmission can be enhanced and the electrolyte and electrode can be given good compatibility. Specifically, the amphiphilic organic molecular particles are mixed with lithium salts and organic polymers in an organic solvent to form a polymer precursor slurry, and finally the stirred slurry is cast in a mold made of polytetrafluoroethylene material, and the organic solvent is completely volatilized in a vacuum environment to obtain a polymer electrolyte membrane integrated with trace amphiphilic molecular fillers. The mass fraction of the amphiphilic molecular filler in the composite solid electrolyte membrane is 0.5wt% to 10wt%.
[0055] The amphiphilic molecular filler particles include at least one of amino acids such as cysteine, glutamic acid, lysine, and asparagine.
[0056] The trace amphiphilic filler integrated composite polymer solid electrolyte of the present invention is formed by filling a pure polymer electrolyte with an amphiphilic filler, wherein the composite polymer electrolyte integrated with trace amphiphilic fillers includes an organic polymer matrix, a lithium salt and an amphiphilic filler. The organic polymer may be at least one of polyethylene oxide PEO, polyethylene glycol PEG, polyvinylidene fluoride PVDF, poly (vinylidene fluoride-co-hexafluoropropylene) PVDF-HFP, and the lithium salt includes at least one of bistrifluoromethanesulfonyl imide lithium LiTFSI, bistrifluoromethanesulfonyl imide lithium salt LiFSI, lithium hexafluorophosphate LiPF6, and lithium perchlorate LiClO4. The polymer and the lithium salt may be preferably polyethylene oxide PEO and bistrifluoromethanesulfonyl imide lithium LiTFSI, respectively. The molar ratio of ethylene oxide monomer [EO] to lithium salt is in the range of (10 to 20):1.
[0057] The following is an exemplary description of the preparation method of the composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers provided by the present invention.
[0058] The polymer solid electrolyte membrane integrated with trace amphiphilic molecular fillers is prepared by solution casting process using amphiphilic organic molecules as polymer electrolyte fillers. As an example, 360 mg of lithium fluoromethanesulfonyl imide LiTFSI and 880 mg of PEO powder (where [EO]: Li +The ratio is in the range of 10 to 20:) is added to 20 mL of acetonitrile solution. Then the amphiphilic filler is added to the solution. The mixture is stirred at room temperature for at least 4 hours to obtain a uniform and transparent precursor slurry. The mixed slurry is then cast on a polytetrafluoroethylene PTFE plate and evaporated at room temperature. Finally, the electrolyte membrane is peeled off from the PTFE mold and vacuum dried at 60°C for at least 24 hours for standby use. The thickness of the composite polymer solid electrolyte membrane integrated with trace amphiphilic fillers can be adjusted as needed by adjusting the slurry volume and the area of the mold, and its thickness can generally be 18 to 100 μm.
[0059] The solid-state lithium metal symmetric battery system provided by the present invention is a battery with lithium metal sheets on both sides. The current density of the lithium deposition and stripping cycle test of the lithium metal symmetric battery system can be 0.1-1.4 mA / cm 2 The deposition or stripping time in each cycle can be 0.5 to 1 h.
[0060] The solid-state lithium metal battery provided by the present invention has a metal lithium sheet as the negative electrode, and the positive electrode can be at least one of ferric trifluoride FeF3, ferrous fluoride FeF2, copper fluoride CuF2, copper hydroxide fluoride CuOHF, carbon-sulfur composite, ferrous disulfide FeS2, lithium manganate LiMn2O4, lithium iron phosphate LiFePO4, lithium cobalt oxide LiCoO2, nickel-rich ternary system and lithium-rich manganese-based solid solution. The composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers is placed between the positive and negative electrodes.
[0061] The invention provides a conversion reaction type large-size fluorine-based solid soft-pack battery based on a composite solid polymer electrolyte integrated with trace amphiphilic molecular fillers, wherein a thin-layer lithium strip (thickness of about 45 μm) is used as the negative electrode, and a positive electrode film contains a fluoride positive electrode (active material), a small amount of conductive carbon, a polymer and a lithium salt. The composite polymer electrolyte integrated with trace amphiphilic molecular fillers is located between the positive and negative electrodes.
[0062] In the present invention, a composite solid electrolyte membrane integrated with trace amphiphilic molecular fillers is obtained by using amphiphilic organic molecules as fillers of polymer electrolytes. Among them, amphiphilic organic molecules can dissolve in the polymer system, produce strong interactions with the polymer, and improve the lithium ion conductivity of the composite polymer. Amphiphilic organic molecules can also promote the movement of anions after the dissociation of the acting lithium salt and the dissociation of the bound lithium salt, and improve the lithium ion migration number of the composite (up to 0.68). In addition, the rich functional groups contained in the trace amphiphilic molecular fillers promote the in-situ formation of a stable solid electrolyte interface phase (SEI) protective layer at the electrolyte / electrode interface. The protective layer synergistically enhances the cycle stability of the symmetric battery. The trace amphiphilic molecular fillers also give lithium iron fluoride conversion batteries excellent rate performance and long-term cycle stability. These batteries can still have a high capacity retention rate after 700 cycles at a rate of 0.5C. In addition, the fluorine-based solid-state soft-pack battery was successfully operated, effectively promoting the future practical application of fluorine-based battery systems.
[0063] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0064] Example
[0065] 1) Preparation of composite polymer solid electrolytes integrated with trace amphiphilic molecular fillers
[0066] The composite solid polymer membrane integrated with trace amphiphilic molecular fillers was prepared by solution casting. First, 360 mg of lithium bis(trifluoromethanesulfonyl)imide LiTFSI and 880 mg of polyethylene oxide PEO powder (where [EO]:Li + The molar ratio is 16:1) is added to 20mL acetonitrile. Then the cysteine particles are added to the solution (the amount of cysteine added in this embodiment is 0.5wt%, 1wt%, 3wt%, 5wt%, and 10wt%, corresponding to 6.2mg, 12.4mg, 37.2mg, 62mg, and 124mg, respectively). The mixture is stirred at room temperature for at least 4h to obtain a uniform transparent solution. The solution is then cast on a polytetrafluoroethylene PTFE plate and evaporated at room temperature. Finally, the electrolyte membrane is peeled off from the PTFE mold and vacuum dried at 60°C for at least 24h, corresponding to the different addition amounts of the above-mentioned cysteine, to obtain a composite polymer solid electrolyte product integrating multiple trace amphiphilic molecular-level fillers.
[0067] Due to the strong interaction between amphiphilic fillers and organic polymers, composite polymers are very easy to achieve ultra-thin manufacturing (18μm thick), such as Figure 1 As shown. Figure 2 The scanning electron microscopy images of the composite polymer solid electrolyte show the potential dissolution of trace amphiphilic fillers in the organic polymer matrix, which is conducive to the penetration of the cross-linked interface.
[0068] 2) Conductivity test of composite polymer solid electrolytes integrated with trace amphiphilic molecular fillers
[0069] SS|PEO-LCy|SS cells were assembled and measured in constant potential mode using a Solartron frequency analyzer (1296-1260) in the frequency range of 1 MHz to 0.1 Hz and 10 data points per decade. The ionic conductivity of the solid electrolyte was measured using an AC perturbation of 10 mV. The solid polymer membrane was cut into discs with a diameter of 17 mm, and two conductive stainless steel electrodes were placed on both sides of the electrolyte membrane. For temperature-dependent measurements, the battery was placed in an oven and impedance tests were performed in the range of 70°C to 30°C with a step size of 10°C. Each temperature point was kept for 1 h to ensure that a steady state was reached. The ionic conductivity (ρ) of the solid polymer electrolyte was calculated by the following formula:
[0070] Where R is the resistance value, L is the film thickness, and S is the contact area of the electrode. Figure 3 The composite electrolyte reinforced with 1 wt% amphiphilic filler has the highest conductivity, which is 2.3×10 -4 S / cm, increased to 5.4×10 at 60℃ -4 S / cm.
[0071] 3) Assembly and testing of solid-state lithium metal symmetric batteries
[0072] The 2025 button cell was assembled in an argon glove box with water and oxygen values less than 0.1 ppm. The charge and discharge tests were performed on a LAND electrochemical workstation at 0.2 mA / cm 2 At a current density of , the battery was first charged at a constant current for 1 hour, and then discharged at a constant current for 1 hour to detect the voltage polarization difference of metal lithium during the deposition / stripping process, and the cycle was carried out in this way. Figure 4As shown, the symmetric battery was tested at a current density of 0.2 mA cm-2 and an area capacity of 0.2 mAh cm-2. It can be seen that the battery based on the pure polymer electrolyte system short-circuited after only about 200 hours of operation. In contrast, the solid-state electrolyte battery based on trace amphiphilic fillers can successfully work stably for more than 1400 hours, and the voltage polarization fluctuation is not obvious, maintained at about 100 mV. In addition, after the solid-state electrolyte battery based on trace amphiphilic fillers is cycled for 120 hours, the morphology of the lithium negative electrode after cycling is observed by SEM imaging, as shown in Figure 5 As shown, unique layered lithium deposition can be observed with a dense and smooth surface, indicating that lithium dendrite growth is effectively suppressed. The higher lithium ion transference number and ionic conductivity in the solid electrolyte integrated with trace amphiphilic molecular fillers are the main reasons for the uniform lithium deposition on the lithium foil surface.
[0073] 4) Preparation and testing of solid-state lithium metal batteries based on composite solid polymer electrolytes integrated with trace amphiphilic molecular fillers:
[0074] 4) a) Preparation of solid positive electrode:
[0075] In order to prepare the positive electrode of the all-solid-state battery, LiTFSI-PEO is introduced into the positive electrode as an ion conductor. In this example, the FeF3 positive electrode is described as the preferred object. In the preparation process of the positive electrode, the active material is mixed with conductive carbon black (Super P), polyethylene oxide (PEO) and bistrifluoromethanesulfonyl imide lithium LiTFSI salt in a weight ratio of 60:12:20:8, and then 12mL of acetonitrile is added to form a uniform mixture. The mixture is stirred at room temperature for 12h and then cast on a carbon-coated aluminum foil. The loading amount of FeF3 is 1mg cm -2 about.
[0076] 4) b) Assembly and testing of solid-state lithium / iron fluoride batteries based on composite solid polymer electrolytes integrated with trace amphiphilic fillers:
[0077] The 2025 button cell was assembled in an argon glove box with water and oxygen values less than 0.1ppm. The cycle performance was tested at 60℃ and different specific currents, and the constant current measurement was performed using a Land battery tester. The voltage range of the Li||FeF3 battery test was 1.2~3.9V. Figure 6 The performance of Li||FeF3 battery after 700 charge and discharge cycles. The battery still has relatively stable cycle performance when cycled to 700 cycles at 0.5C, and the coulombic efficiency is close to 100%. During the long cycle process, the two-stage discharge platform can be well maintained, and the high capacity is still maintained after 700 cycles. Figure 7The typical two-stage platform during the charge and discharge process of Li||FeF3 batteries is demonstrated, and the two-stage discharge platform can be well preserved during long-term cycling.
[0078] 5) Preparation and testing of soft-pack Li||FeF3 batteries based on composite polymer electrolytes integrated with trace amphiphilic molecular fillers:
[0079] The preparation and measurement process of solid-state Li||FeF3 soft-pack battery is as follows: the prepared FeF3-based positive electrode (single-sided coating, similar to the preparation process of the aforementioned button battery) is cut into 6×4 cm 2 The sheet has an active material loading of about 1 mg cm-2. The lithium foil is cut into slightly larger sizes, about 6.2 × 4.2 cm 2 , the PEO-LCy composite polymer film was cut into larger sizes of 6.5 × 4.5 cm 2 , to completely separate the FeF3 cathode and the lithium metal anode. These sheets were stacked and assembled into soft-pack batteries and electrochemically tested after being placed in an oven at 60°C for 6 h. Figure 8 The actual picture of Li||FeF3 soft pack battery is shown. The soft pack battery has a current density of 100mA g -1 Up to 550mAh g -1 The discharge capacity of the battery was 350 mAh g after 200 and 500 cycles, respectively. -1 ,like Fig. 9 In addition, the soft pack battery was subjected to an abuse test. Fig.10 It can be seen that the soft-pack battery can provide a stable current to illuminate the LED bulb even if it is subjected to different degrees of abuse, including bending, folding, puncture, and cutting. These treatments demonstrate that the soft-pack Li||FeF3 battery with a composite polymer electrolyte integrated with trace amphiphilic fillers has good safety and practicality under extreme conditions.
[0080] Comparative Example
[0081] 1) Preparation of PEO polymer electrolyte:
[0082] The composite electrolyte membrane was prepared by solution casting. First, 360 mg of lithium bis(trifluoromethanesulfonyl)imide LiTFSI and 880 mg of PEO powder (where [EO]:Li + The mixture was stirred at room temperature for at least 4 hours to obtain a milky white slurry solution. The solution was then cast on a polytetrafluoroethylene (PTFE) plate and evaporated at room temperature. Finally, the electrolyte membrane was peeled off from the PTFE mold and vacuum dried at 60°C for at least 24 hours for use.
[0083] 2) Assembly and testing of lithium / ferric fluoride batteries with PEO polymer electrolyte:
[0084] The 2025 button cell was assembled in an argon glove box with a water and oxygen value of less than 0.1ppm. The specific process is to attach a 10mm diameter lithium metal sheet and a positive electrode sheet loaded with active substances on both sides of a 16mm diameter PEO polymer film to assemble a lithium metal battery. The battery was then tested for electrochemical cycling performance at 60°C and different current densities in a LAND electrochemical workstation. Fig.11 This is a graph of the cycling performance of a Li||FeF3 battery with a pure PEO polymer solid electrolyte system. After about 20 stable cycles, the coulombic efficiency of the full battery deteriorates and the battery gradually necrotizes.
[0085] It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the application.
Claims
1. A composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers, characterized in that: The invention comprises an organic polymer matrix, and lithium salt and amphiphilic molecular filler dispersed in the organic polymer matrix.
2. A composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers as claimed in claim 1, characterized in that: The organic polymer comprises at least one of polyethylene oxide, polyacrylonitrile, polyethylene glycol, polyvinylidene fluoride, and poly(vinylidene fluoride-co-hexafluoropropylene); The lithium salt includes at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium hexafluorophosphate, and lithium perchlorate.
3. A composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers as claimed in claim 1, characterized in that: The mass fraction of the amphoteric molecular filler in the composite polymer solid electrolyte is 0.5wt% to 10wt%.
4. A composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers as claimed in claim 1, characterized in that: The amphiphilic molecular grade filler includes at least one of cysteine, glutamic acid, lysine and asparagine.
5. A composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers as claimed in claim 1, characterized in that: The molar mass of the organic polymer is calculated based on the molar mass of the polymerized monomer used to form the organic polymer, and the molar ratio of the organic polymer monomer to the lithium salt is (10-20):
1.
6. A composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers as claimed in claim 1, characterized in that: The thickness of the composite solid electrolyte integrated with trace amphiphilic molecular fillers is 18-100 μm.
7. A method for preparing a composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: S1, adding an organic polymer, a lithium salt and amphiphilic molecular filler particles into an organic solvent, and mixing to obtain a mixed slurry; S2, pouring the obtained mixed slurry on a substrate to form a composite polymer film precursor; S3. Heat the substrate coated with the composite polymer film precursor to 40-80° C. under vacuum conditions, keep it warm for at least 24 hours, and then air-cool it to room temperature to obtain the composite polymer solid electrolyte integrated with the trace amphiphilic molecular-level filler.
8. The method for preparing a composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers as claimed in claim 7, characterized in that: The organic solvent is one of acetonitrile, dimethylformamide and N-methylpyrrolidone; The mixing method is stirring, and the stirring is stirring at room temperature to 60° C. for 4 to 8 hours.
9. The method for preparing a composite polymer solid electrolyte integrated with trace amphiphilic molecular fillers as claimed in claim 7, characterized in that: The substrate is a polytetrafluoroethylene plastic plate.
10. A lithium metal symmetric battery system based on a composite polymer solid electrolyte, characterized in that: The lithium metal symmetric battery system comprises a composite polymer solid electrolyte integrated with a trace amount of amphiphilic molecular filler according to any one of claims 1 to 6, and metal lithium sheets located on both sides of the composite polymer solid electrolyte integrated with a trace amount of amphiphilic molecular filler.
11. A solid-state lithium metal battery based on a composite polymer solid electrolyte, characterized in that: The solid-state lithium metal battery comprises a positive electrode, a negative electrode, and a composite polymer solid electrolyte integrated with a trace amount of amphiphilic molecular-level filler according to any one of claims 1 to 6 and located between the positive electrode and the negative electrode.
12. A solid-state lithium metal battery based on a composite polymer solid electrolyte according to claim 11, characterized in that: The negative electrode is a metal lithium sheet, and the positive electrode is at least one of ferric trifluoride, ferrous fluoride, iron oxyfluoride, copper fluoride, copper hydroxide fluoride, carbon-sulfur composite, ferrous disulfide, lithium manganate, lithium iron phosphate, lithium cobalt oxide, nickel-rich ternary system and lithium-rich manganese-based solid solution.
13. A solid-state lithium / fluoride battery in a soft-pack configuration based on a composite polymer solid electrolyte, characterized in that: The soft-pack battery comprises a positive electrode, a negative electrode, and a composite polymer solid electrolyte integrated with the trace amount of amphiphilic molecular-level filler as claimed in any one of claims 1 to 6 located between the positive electrode and the negative electrode.
14. A solid-state lithium / fluoride battery in a soft-pack configuration based on a composite polymer solid electrolyte as claimed in claim 13, characterized in that: The negative electrode is a thin-layer metallic lithium, and the positive electrode is at least one of ferric trifluoride, ferrous fluoride, iron oxyfluoride, copper fluoride, and copper hydroxide fluoride.