Nonaqueous secondary battery and method for manufacturing nonaqueous secondary battery

By adjusting the unit compression parameters of the non-aqueous secondary battery, the thickness expansion of the battery pack during expansion is suppressed, and the Li precipitation resistance is improved, and the problems of spacer deformation and electrolyte deterioration in the prior art are solved, thus achieving more stable battery structure and performance.

CN119009147APending Publication Date: 2024-11-22TOYOTA BATTERY CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410575838.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2024-05-10
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When the electrode group expands, the spacer is prone to deformation, resulting in difficult suppression of expansion of unit thickness, and deterioration of the impregnation property of the electrolyte, resulting in a decrease in Li precipitation resistance.

Method used

By adjusting the unit compression parameters in a non-aqueous secondary battery, it is made to be above 0.000 and below 0.007, the unit compression force calculated by combining the spring constant by multiplying the differential pressure of the housing with the atmospheric pressure and the area of ​​the flat part of the electrode body by combining the spring constant. , suppress the expansion of the unit thickness and maintain the reduced pressure state of the electrolyte.

Benefits of technology

The expansion of the unit thickness when unconstrained is effectively suppressed, and the Li precipitation resistance is improved, and the impregnation property of the electrolyte solution to the electrode body is prevented.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009147A_ABST
    Figure CN119009147A_ABST
Patent Text Reader

Abstract

The invention provides a non-aqueous secondary battery and a method for manufacturing the non-aqueous secondary battery. The non-aqueous secondary battery suppresses the expansion of the cell thickness when the non-constraint is not carried out. A non-aqueous secondary battery is provided with: an electrode body in which a positive electrode sheet and a negative electrode sheet are laminated with a separator therebetween; a non-aqueous electrolyte solution; and a battery case in which the electrode body and the non-aqueous electrolyte solution are housed. In the non-aqueous secondary battery, a cell compression parameter obtained by dividing a cell compression force obtained from the product of the surface area of the flat portion of the electrode body and the differential pressure of the internal pressure of the battery case with respect to atmospheric pressure by the spring constant of the battery case (11) is 0.000-0.007.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a non-aqueous secondary battery and a method for manufacturing the non-aqueous secondary battery. Background Art

[0002] The battery pack described in Patent Document 1 includes a plurality of arranged single cells and a separator sandwiched between the single cells. The single cell includes an electrode group in which a positive electrode and a negative electrode are stacked oppositely with a separator therebetween, and a square casing for housing the electrode group. The electrode group expands in the stacking direction as it is charged and discharged. The negative electrode plate described in Patent Document 1 is harder than the separator. Therefore, if the electrode group expands, the separator, which is softer than the negative electrode plate, deforms and absorbs the strain. Prior art literature Patent Literature

[0003] Patent Document 1: Japanese Patent Application Publication No. 2017-84550 Summary of the invention Problems to be solved by the invention

[0004] However, in the battery pack (cell) described in Patent Document 1, the hardness of the negative electrode plate needs to be set according to the separator, and therefore, it is required to suppress the expansion of the cell thickness when it is not constrained. Means for solving problems

[0005] A non-aqueous secondary battery in one embodiment of the present invention comprises an electrode body formed by stacking positive and negative electrode sheets with separators therebetween, a non-aqueous electrolyte, and a shell for accommodating the electrode body and the non-aqueous electrolyte, wherein a cell compression parameter obtained by dividing a cell compression force obtained by multiplying the differential pressure of the internal pressure of the shell with respect to atmospheric pressure by the area of ​​a flat portion of the electrode body by a spring constant of the shell is greater than 0.000 and less than 0.007.

[0006] A method for manufacturing a non-aqueous secondary battery in one embodiment of the present invention comprises an electrode body formed by stacking a positive electrode sheet and a negative electrode sheet with a separator therebetween, a non-aqueous electrolyte, and a shell for accommodating the electrode body and the non-aqueous electrolyte, wherein a cell compression parameter obtained by dividing a cell compression force obtained by multiplying the pressure difference between the internal pressure of the shell and the atmospheric pressure by the area of ​​the flat portion of the electrode body by a spring constant of the shell is adjusted to be greater than 0.000 and less than 0.007. Effects of the Invention

[0007] According to one aspect of the present disclosure, it is possible to suppress expansion of the cell thickness when not constrained. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 It is a perspective view showing a schematic structure of a unit cell of one embodiment of a non-aqueous secondary battery. Figure 2 This is a diagram showing a part of an electrode body of an embodiment of a non-aqueous secondary battery. Figure 3 This is a cross-sectional view of a unit cell of one embodiment of a non-aqueous secondary battery. Figure 4 This is a graph showing the cell thickness and Li precipitation resistance in an unconstrained state with respect to the cell compression parameter of a nonaqueous secondary battery according to one embodiment of the nonaqueous secondary battery. Figure 5 This is a table showing examples and comparative examples of non-aqueous secondary batteries. DETAILED DESCRIPTION

[0009] [Present Embodiment] The following reference Figure 1 to Figure 4 An embodiment of a nonaqueous secondary battery and a method for manufacturing the nonaqueous secondary battery will be described. A lithium ion secondary battery will be described as an example of a nonaqueous secondary battery.

[0010] [Lithium ion secondary battery 10] like Figure 1 As shown, the lithium ion secondary battery 10 is a unit cell that is enclosed in a case made of resin or metal in a state where a plurality of lithium ion secondary batteries 10 are combined to form a battery pack. The battery pack is used in a hybrid vehicle or an electric vehicle.

[0011] The lithium-ion secondary battery 10 includes a battery case 11 and a cover 12. The battery case 11 is a rectangular parallelepiped having an opening on the upper side. The cover 12 seals the opening of the battery case 11. The battery case 11 and the cover 12 are made of metal such as aluminum or an aluminum alloy. In the lithium-ion secondary battery 10, the cover 12 is mounted on the battery case 11 to form a sealed battery container.

[0012] The positive external terminal 13A and the negative external terminal 13B are provided on the cover body 12. The positive external terminal 13A and the negative external terminal 13B are used for charging and discharging of electric power. The electrode body 20 is housed inside the battery case 11. An external insert film (not shown) is inserted between the battery case 11 and the electrode body 20. The positive electrode side collector 20A, which is the end of the positive electrode side in the electrode body 20, is electrically connected to the positive electrode external terminal 13A via the positive electrode side collector component 14A. The negative electrode side collector 20B, which is the end of the negative electrode side in the electrode body 20, is electrically connected to the negative electrode external terminal 13B via the negative electrode side collector component 14B. In addition, the non-aqueous electrolyte is injected into the battery case 11 from an injection hole not shown in the figure. It should be noted that the shapes of the positive electrode external terminal 13A and the negative electrode external terminal 13B are not limited to. Figure 1 The shape shown can be any shape.

[0013] [Electrode body 20] like Figure 2 As shown, the electrode body 20 is a flat wound body formed by stacking the long strip positive electrode sheet 21 and the negative electrode sheet 24 with the separator 27 interposed therebetween and winding the obtained laminated body. The positive electrode sheet 21, the negative electrode sheet 24 and the separator 27 are stacked in such a manner that the long side directions of each are consistent with the longitudinal direction D1. The laminated body before winding is stacked in the order of the positive electrode sheet 21, the separator 27, the negative electrode sheet 24 and the separator 27.

[0014] [Positive electrode sheet 21] The positive electrode sheet 21 includes a positive electrode collector 22 and a positive electrode composite material layer 23. The positive electrode collector 22 is a positive electrode substrate formed in a long foil shape. The positive electrode composite material layer 23 is provided on two opposite surfaces of the positive electrode collector 22. The positive electrode collector 22 has a positive electrode side uncoated portion 22A at one end in the width direction D2 where the positive electrode composite material layer 23 is not formed and the positive electrode collector 22 is exposed.

[0015] A metal foil made of aluminum or an alloy containing aluminum as a main component is used as the positive electrode current collector 22. The positive electrode current collector 22 functions as a current collector in the positive electrode. The positive electrode side uncoated portion 22A of the positive electrode current collector 22 is formed by pressing the opposing surfaces together in the state of the wound body to form a positive electrode side current collecting portion 20A.

[0016] The positive electrode composite material layer 23 is a solidified body of a liquid positive electrode composite material paste. The positive electrode composite material paste contains a positive electrode active material, a positive electrode solvent, a positive electrode conductive material, and a positive electrode binding material. The positive electrode composite material layer 23 is formed by drying the positive electrode composite material paste and vaporizing the positive electrode solvent. Therefore, the positive electrode composite material layer 23 contains a positive electrode active material, a positive electrode conductive material, and a positive electrode binding material.

[0017] The positive electrode active material uses a lithium-containing composite oxide that can absorb and release lithium ions as charge carriers in the lithium-ion secondary battery 10. The lithium-containing composite oxide is an oxide containing lithium and other metal elements other than lithium. The other metal elements other than lithium are, for example, at least one selected from the group consisting of nickel, cobalt, manganese, vanadium, magnesium, molybdenum, niobium, titanium, tungsten, aluminum, and iron contained in the lithium-containing composite oxide in the form of iron phosphate.

[0018] For example, the lithium-containing composite oxide is lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), and lithium manganese oxide (LiMn2O4). For example, the lithium-containing composite oxide is a ternary lithium-containing composite oxide containing nickel, cobalt, and manganese, such as lithium nickel cobalt manganese oxide (LiNiCoMnO2). For example, the lithium-containing composite oxide is lithium iron phosphate (LiFePO4).

[0019] The positive electrode solvent uses NMP (N-methyl-2-pyrrolidone) solution as an example of an organic solvent. As the positive electrode conductive material, for example, carbon black such as acetylene black and Ketjen black, carbon fibers such as carbon nanotubes and carbon nanofibers, and graphite are used. The positive electrode binder is an example of a resin component contained in the positive electrode composite material paste. For example, the positive electrode binder uses polyvinylidene fluoride (PVDF), polyvinyl alcohol (PVA), styrene butadiene rubber (SBR), etc.

[0020] It should be noted that the positive electrode sheet 21 may have an insulating layer at the boundary between the positive electrode side uncoated portion 22A and the positive electrode composite material layer 23. The insulating layer includes an inorganic component having insulating properties and a resin component that functions as a binding material. The inorganic component is at least one selected from the group consisting of powdered boehmite, titanium dioxide and aluminum oxide. The resin component is at least one selected from the group consisting of PVDF, PVA, and acrylic acid.

[0021] [Negative electrode 24] The negative electrode sheet 24 includes a negative electrode collector 25 and a negative electrode composite material layer 26. The negative electrode collector 25 is a negative electrode substrate formed in a long foil shape. The negative electrode composite material layer 26 is provided on two opposite surfaces of the negative electrode collector 25. The negative electrode collector 25 has a negative electrode side uncoated portion 25A where the negative electrode composite material layer 26 is not formed and the negative electrode collector 25 is exposed at an end portion located opposite to the positive electrode side uncoated portion 22A as one end in the width direction D2.

[0022] A metal foil made of copper or an alloy containing copper as a main component is used as the negative electrode current collector 25. The negative electrode current collector 25 functions as a current collector in the negative electrode. The negative electrode side uncoated portion 25A is formed by pressing the opposing surfaces of the wound body together to form the negative electrode side current collector 20B.

[0023] The negative electrode composite material layer 26 is a solidified body of a liquid negative electrode composite material paste. The negative electrode composite material paste contains a negative electrode active material, a negative electrode solvent, a negative electrode thickening material, and a negative electrode binding material. The negative electrode composite material layer 26 is formed by drying the negative electrode composite material paste and vaporizing the negative electrode solvent. Therefore, the negative electrode composite material layer 26 contains a negative electrode active material, and a negative electrode thickening material and a negative electrode binding material as additives. It should be noted that the negative electrode composite material layer 26 may further contain additives such as conductive materials.

[0024] The negative electrode active material is a material that can absorb and release lithium ions. Examples of the negative electrode active material include carbon materials such as graphite, difficult-graphitizable carbon, easy-graphitizable carbon, and carbon nanotubes. As for the negative electrode solvent, water is used as an example. As for the negative electrode thickening material, CMC (carboxymethyl cellulose) as a thickening material containing sodium salt can be used as an example. The negative electrode binding material can use the same material as the positive electrode binding material. As for the negative electrode binding material, SAR (styrene acrylic acid copolymer) as a binding material containing sodium salt can be used as an example.

[0025] [Spacer 27] The separator 27 prevents contact between the positive electrode sheet 21 and the negative electrode sheet 24 and holds the nonaqueous electrolyte between the positive electrode sheet 21 and the negative electrode sheet 24. When the electrode body 20 is immersed in the nonaqueous electrolyte, the nonaqueous electrolyte permeates from the ends of the separator 27 in the width direction D2 to the center.

[0026] The separator 27 is a nonwoven fabric made of polypropylene, etc. As the separator 27, for example, a porous polymer film such as a porous polyethylene film, a porous polyolefin film, a porous polyvinyl chloride film, or an ion conductive polymer electrolyte membrane can be used.

[0027] [Non-aqueous electrolyte] The non-aqueous electrolyte is a composition containing a supporting salt in a non-aqueous solvent. As the non-aqueous solvent, one or more materials selected from the group consisting of propylene carbonate, ethylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, etc. can be used. In addition, as the supporting salt, one or more lithium compounds (lithium salts) selected from LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC4F9SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, LiI, LiBOB (lithium bis(oxalatoborate)), etc. can be used.

[0028] In this embodiment, ethylene carbonate is used as a non-aqueous solvent. LiBOB, a lithium salt, is added to the non-aqueous electrolyte as a coating forming agent. For example, LiBOB is added to the non-aqueous electrolyte in such a manner that the concentration of LiBOB in the non-aqueous electrolyte is greater than or equal to 0.001 and less than or equal to 0.1 [mol / L].

[0029] [Manufacturing method] Next refer to Figure 3 and Figure 4 A method for manufacturing the lithium ion secondary battery 10 will be described.

[0030] like Figure 3As shown, if the thickness T of the electrode body 20 exceeds the inner dimension W of the battery shell 11, the thickness of the unit cell expands. Therefore, in order to prevent the thickness of the unit cell from expanding, the unit compression parameter is set to be greater than 0.000 and less than 0.007. The unit compression parameter is obtained by dividing the unit compression force by the unit spring constant. The unit spring constant is calculated based on the thickness deformation from 2kN to 5kN when the battery cell is compressed using Autograph (precision universal testing machine). The unit compression parameter is shown in formula (1). The unit compression force is obtained by multiplying the differential pressure of the internal pressure of the battery shell 11 relative to the atmospheric pressure by the flat area of ​​the electrode body 20. The unit compression force is shown in formula (2). The flat area of ​​the electrode body 20 is obtained by multiplying the positive electrode coating width by the length of the electrode body plane. The flat area of ​​the electrode body 20 is shown in formula (3). The length of the electrode body plane, for example, uses the innermost length of the length direction D1 of the positive electrode in the electrode body 20 (i.e., the innermost positive electrode length).

[0031] Unit compression parameter = unit compression force ÷ unit spring constant [kN / mm] ···Equation (1) Cell compression force = - cell internal pressure [MPa] × electrode body flat area [mm 2 ]···Formula (2) Electrode body flat area = positive electrode coating width [mm] × electrode body flat surface length [mm] ···Formula (3)

[0032] like Figure 4 As shown, by making the cell compression parameter greater than 0.000 and exerting a cell compression force based on atmospheric pressure, the expansion of the cell thickness when not constrained can be suppressed. The cell thickness when not constrained is the thickness measured by the way that the measuring element of the digital indicator (for example, pressing at 1.5N) contacts the maximum value of the convex position on the side of the battery cell. The cell thickness when there is no expansion is the sum of the plate thickness (both sides) of the battery case 11, the thickness (both sides) of the external insert film 15, and the thickness of the electrode body 20 (refer to Figure 3 ).

[0033] In addition, if the cell internal pressure decreases and the cell compression parameter is 0.007 or more, the cell is in a decompressed state, and the electrolyte impregnation into the electrode body 20 is deteriorated. If the electrolyte impregnation is deteriorated, the film formation on the negative electrode becomes uneven, and the Li precipitation resistance is reduced. Regarding the Li precipitation resistance, the Li precipitation limit current value when the cell compression parameter is 0.000 is taken as 100, and the Li precipitation resistance in each battery cell is indexed.

[0034] Therefore, by setting the cell compression parameter to 0.000 or more and 0.007 or less, it is possible to suppress the variation in the cell thickness when not constrained, and to suppress the reduction in Li precipitation resistance caused by making the cell interior a decompressed state.

[0035] Next, the effects of this embodiment will be described. (1) By making the cell compression parameter greater than 0.000, the cell compression force based on atmospheric pressure is exerted, which can suppress the expansion of the cell thickness when not constrained. In addition, by making the cell compression parameter less than 0.007, the cell is in a decompressed state, which can suppress the deterioration of the electrolyte's penetration into the electrode body 20.

[0036] (Other embodiments) The above-mentioned embodiment can be implemented by modification as follows. The above-mentioned embodiment and the following modification examples can be implemented in combination with each other within the scope that there is no technical contradiction.

[0037] In the above-mentioned embodiment, the unit spring constant can be adjusted to be soft by increasing the number of spacers. In the above embodiment, the opening of the battery case 11 is sealed with the cover 12 immediately after the electrolyte is placed in the battery case 11, thereby sealing the battery case 11, thereby making the pressure inside the battery cell negative. In addition, by increasing the space between the electrode body 20 of the battery case 11 and the cover 12 and allowing the electrolyte to penetrate into the electrode body 20, the pressure inside the battery cell can be negative.

[0038] In the above embodiment, the positive electrode sheet 21 and the negative electrode sheet 24 are stacked with the separator 27 interposed therebetween, and the resulting stack is wound to form the electrode body 20. However, a plurality of positive electrode sheets 21 and a plurality of negative electrode sheets 24 may be alternately stacked with the separator 27 interposed therebetween to form a stack to form the electrode body.

[0039] The lithium ion secondary battery 10 can be mounted on a computer or other electronic device in addition to an automatic conveyor, a special vehicle for loading and unloading, an electric vehicle, a hybrid vehicle, etc., and can also constitute other systems. For example, it can be installed in a mobile body such as a ship or an aircraft, or it can be a power supply system that supplies power from a power plant to a building or a home where the secondary battery is installed via a substation.

[0040] [Example] Next refer to Figure 5 Examples and comparative examples of the lithium ion secondary battery 10 will be described. Note that these examples and comparative examples do not limit the method for producing the non-aqueous secondary battery.

[0041] In the following, Figure 5As shown, the lithium ion secondary batteries 10 of the examples and comparative examples were prepared by changing the combination of the cell internal pressure, the positive electrode coating width, the innermost positive electrode length, and the cell spring constant. In addition, the cell compression parameter was calculated for each example and each comparative example, and the cell thickness [mm] and the precipitation limit current [%] when not constrained were evaluated.

[0042] [Comparative Example 1] The cell internal pressure was set to 0.030 [MPa] higher than the atmospheric pressure, and the flat area of ​​the electrode body was set to 3632 [mm 2 ], the unit spring constant is 37.0 [kN / mm], and the unit compression parameter is -0.003.

[0043] [Comparative Example 2] The cell internal pressure was set to 0.028 [MPa] which is greater than the atmospheric pressure, and the flat area of ​​the electrode body was set to 3636 [mm 2 ], the unit spring constant is 40.6 [kN / mm], and the unit compression parameter is -0.002.

[0044] [Comparative Example 3] The pressure inside the cell was set to 0.023 [MPa] which is greater than the atmospheric pressure, and the flat area of ​​the electrode body was set to 3612 [mm 2 ], the unit spring constant is 28.5 [kN / mm], and the unit compression parameter is -0.003.

[0045] [Comparative Example 4] The cell internal pressure was set to 0.019 [MPa] higher than the atmospheric pressure, and the flat area of ​​the electrode body was set to 3620 [mm 2 ], the unit spring constant is 40.6 [kN / mm], and the unit compression parameter is -0.002.

[0046] [Comparative Example 5] The cell internal pressure was set to 0.013 [MPa] higher than the atmospheric pressure, and the flat area of ​​the electrode body was set to 3608 [mm 2 ], the unit spring constant is 23.6 [kN / mm], and the unit compression parameter is -0.002.

[0047] [Comparative Example 6] The cell internal pressure was set to -0.050 [MPa] which is less than the atmospheric pressure, and the flat area of ​​the electrode body was set to 4450 [mm 2 ], the unit spring constant is 25.2 [kN / mm], and the unit compression parameter is 0.009.

[0048] [Example 1] The cell internal pressure was set to -0.004 [MPa], which is less than the atmospheric pressure, and the flat area of ​​the electrode body was set to 3620 [mm 2 ], the unit spring constant is 24.5 [kN / mm], and the unit compression parameter is 0.001.

[0049] [Example 2] The cell internal pressure was set to -0.002 [MPa] less than the atmospheric pressure, and the flat area of ​​the electrode body was set to 3620 [mm 2 ], the unit spring constant is 39.3 [kN / mm], and the unit compression parameter is 0.000.

[0050] [Example 3] The cell internal pressure was set to -0.010 [MPa], which is less than the atmospheric pressure, and the flat area of ​​the electrode body was set to 3636 [mm 2 ], the unit spring constant is 40.6 [kN / mm], and the unit compression parameter is 0.001.

[0051] [Example 4] The cell internal pressure was set to -0.040 [MPa], which is less than the atmospheric pressure, and the flat area of ​​the electrode body was set to 4463 [mm 2 ], the unit spring constant is 25.3 [kN / mm], and the unit compression parameter is 0.007.

[0052] [evaluate] The cell thickness [mm] and the precipitation limiting current [%] of each of the above-mentioned examples and comparative examples were evaluated when the cell thickness was not constrained. The cell thickness in the non-expanded state when the cell was not constrained was 12.50 [mm].

[0053] In Comparative Examples 1 to 5, where the cell internal pressure is greater than the atmospheric pressure, the cell thickness when not constrained is greater than 12.50 [mm]. On the other hand, in Comparative Example 6 and Examples 1 to 4, where the cell internal pressure is less than the atmospheric pressure, the cell thickness when not constrained is approximately 12.50 [mm] or less. Therefore, it is preferred that the cell internal pressure is less than the atmospheric pressure and the cell compression parameter is greater than 0.000.

[0054] In Comparative Examples 1 to 5 and Examples 1 to 4, where the cell compression parameter was 0.007 or less, the precipitation limiting current was 100.0% [%. In Comparative Example 6, where the cell compression parameter was 0.009, which was greater than 0.007, the precipitation limiting current was 85.6% [%.] Therefore, it is preferred that the cell compression parameter be 0.007 or less. Examples 1 to 4 obtained excellent results.

Claims

1. A non-aqueous secondary battery comprising an electrode body formed by stacking a positive electrode sheet and a negative electrode sheet with a separator therebetween, a non-aqueous electrolyte, and a casing for accommodating the electrode body and the non-aqueous electrolyte, wherein: A cell compression parameter obtained by dividing a cell compression force obtained by multiplying a differential pressure of the inner pressure of the case with respect to atmospheric pressure by an area of ​​a flat portion of the electrode body by a spring constant of the case is 0.000 or more and 0.007 or less.

2. A method for manufacturing a non-aqueous secondary battery, the non-aqueous secondary battery comprising an electrode body formed by stacking a positive electrode sheet and a negative electrode sheet with a separator therebetween, a non-aqueous electrolyte, and a casing for accommodating the electrode body and the non-aqueous electrolyte, wherein: A cell compression parameter obtained by dividing a cell compression force obtained by multiplying the differential pressure of the case with respect to the atmospheric pressure by the flat portion area of ​​the electrode body by a spring constant of the case is adjusted to be 0.000 or more and 0.007 or less.