Aqueous nickel-zinc secondary battery negative pole piece and aqueous nickel-zinc secondary battery

By using a hydrophobic layer composed of small-particle polyether ether ketone and large-particle polytetrafluoroethylene on the negative electrode sheet of the aqueous nickel-zinc secondary battery, the problem of corrosion and hydrogen analysis of zinc negative electrode is solved, and the significant improvement of the hydrogen analysis of zinc negative electrode is significantly improved. The cycle life and storage performance of nickel-zinc secondary batteries are provided.

CN119009186APending Publication Date: 2024-11-22SHENZHEN HIGHPOWER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411190984.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The contact between the zinc negative electrode and the alkaline electrolyte leads to zinc dendrites, surface passivation and corrosion of hydrogen analysis, limiting the cycleability and storageability of nickel-zinc secondary batteries and reducing the cycle life performance.

Method used

In the negative electrode sheet of the aqueous nickel-zinc secondary battery, a hydrophobic layer is used to separate the contact between the negative electrode material layer and the electrolyte solution. The hydrophobic layer is composed of small-particle polyether ether ketone and large-particle polytetrafluoroethylene. By spraying and Rolling pressure is formed to improve the bonding strength and hydrophobicity of the hydrophobic layer and prevent the occurrence of corrosion and hydrogen evolution.

Benefits of technology

Effectively reduce or even avoid corrosion of zinc negative electrode, improve the cycle life and storage performance of aqueous nickel-zinc secondary batteries, and significantly extend the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009186A_ABST
    Figure CN119009186A_ABST
Patent Text Reader

Abstract

The invention relates to a negative pole piece of a water-based nickel-zinc secondary battery and the water-based nickel-zinc secondary battery. The negative pole piece of the aqueous nickel-zinc secondary battery comprises a current collector, a negative pole material layer arranged on at least one side of the current collector, and a hydrophobic layer coating the negative pole material layer, wherein the hydrophobic layer is used for isolating the contact between the negative pole material layer and an electrolyte; wherein the hydrophobic layer comprises a hydrophobic material, the hydrophobic material comprises a first type of hydrophobic material and a second type of hydrophobic material, the particle size of the first type of hydrophobic material is smaller than that of the second type of hydrophobic material, and the first type of hydrophobic material comprises polyether-ether-ketone. According to the scheme provided by the invention, the corrosion hydrogen evolution of the active substance of the negative pole piece can be effectively reduced or even avoided, the long storage performance and the cycle life performance of the water-based nickel-zinc secondary battery are considered, and the cycle life performance of the water-based nickel-zinc secondary battery is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of nickel-zinc batteries, and in particular to a negative electrode sheet of an aqueous nickel-zinc secondary battery and an aqueous nickel-zinc secondary battery. Background Art

[0002] In recent years, with the increasing application of lithium-ion batteries in energy storage devices, fire accidents caused by lithium-ion batteries have become more and more frequent, attracting widespread attention. Aqueous nickel-zinc secondary batteries have received extensive attention due to their rich raw materials, high energy density, and high safety. Among them, nickel-zinc secondary batteries stand out for their excellent rate performance and environmental friendliness.

[0003] Although the positive electrode of nickel-zinc secondary batteries has been studied quite maturely, the exploration of zinc negative electrodes is still in its infancy. When the zinc negative electrode contacts the alkaline electrolyte, problems such as zinc dendrites, surface passivation, and continuous corrosion and hydrogen evolution during storage and circulation will occur. Among them, corrosion and hydrogen evolution will cause the battery shell to swell and grow higher, or even leak, which seriously limits the recyclability and storability of nickel-zinc secondary batteries, and reduces the long storage performance and cycle life performance of nickel-zinc secondary batteries. Summary of the invention

[0004] In order to solve or partially solve the problems existing in the related art, the present application provides an aqueous nickel-zinc secondary battery negative electrode plate and an aqueous nickel-zinc secondary battery, which can effectively reduce or even avoid the corrosion and hydrogen evolution of the active material of the negative electrode plate, take into account the long storage performance and cycle life performance of the aqueous nickel-zinc secondary battery, and significantly improve the cycle life performance of the aqueous nickel-zinc secondary battery.

[0005] The first aspect of the present application provides a negative electrode plate for an aqueous nickel-zinc secondary battery. It comprises a current collector, a negative electrode material layer disposed on at least one side of the current collector, and a hydrophobic layer covering the negative electrode material layer, wherein the hydrophobic layer is used to isolate the contact between the negative electrode material layer and the electrolyte; wherein, The hydrophobic layer includes a hydrophobic material, which includes a first type of hydrophobic material and a second type of hydrophobic material. The particle size of the first type of hydrophobic material is smaller than that of the second type of hydrophobic material. The first type of hydrophobic material includes polyetheretherketone.

[0006] Preferably, the second type of hydrophobic material includes polymethyl methacrylate and / or fluoroplastic.

[0007] Preferably, the fluoroplastic includes one or more of polytetrafluoroethylene, fluorinated ethylene propylene copolymer, ethylene-tetrafluoroethylene copolymer, and fluoroplastic.

[0008] Preferably, the hydrophobic material and a set solvent are mixed in a set mass ratio to prepare a hydrophobic liquid, the hydrophobic liquid is sprayed on the negative electrode material layer in a set spraying amount, and the hydrophobic layer is formed on the surface of the negative electrode material layer after drying and rolling.

[0009] Preferably, the mass ratio of the hydrophobic material to the set solvent is (1:19)-(1:10).

[0010] Preferably, the second type of hydrophobic material is polytetrafluoroethylene; wherein, In 100 grams of the hydrophobic material, the mass percentage ratio of the polyetheretherketone to the polytetrafluoroethylene is in the range of (20%:80%) to (40%:60%).

[0011] Preferably, the particle size of the polyetheretherketone is 2 μm-5 μm, and the particle size of the polytetrafluoroethylene is 20 μm-30 μm.

[0012] Preferably, the set spraying amount is 5g / m 2 -15g / m 2 ; Preferably, the set spraying amount is 5g / m 2 -10g / m 2 .

[0013] Preferably, the rolling pressure is 1 MPa-5 MPa.

[0014] A second aspect of the present application provides an aqueous nickel-zinc secondary battery, which includes a positive electrode plate, an electrolyte, a separator, and the negative electrode plate as described above.

[0015] The technical solution provided by this application may have the following beneficial effects: The technical solution of the present application is that the negative electrode plate of an aqueous nickel-zinc secondary battery includes a current collector, a negative electrode material layer arranged on at least one side of the current collector, and a hydrophobic layer coating the negative electrode material layer, the hydrophobic layer is used to isolate the contact between the negative electrode material layer and the electrolyte; wherein the hydrophobic layer includes a hydrophobic material, the hydrophobic material includes a first type of hydrophobic material and a second type of hydrophobic material, the particle size of the first type of hydrophobic material is smaller than the particle size of the second type of hydrophobic material, the first type of hydrophobic material includes polyetheretherketone, by doping the first type of hydrophobic material polyetheretherketone with a large particle size of the second type of hydrophobic material, the bonding strength and hydrophobicity of the hydrophobic layer can be improved, so that the hydrophobic layer has stronger hydrophobicity and better bonding, and the bonding strength between the hydrophobic layer and the negative electrode material layer is improved, and the hydrophobic layer including the first type of hydrophobic material polyetheretherketone and the second type of hydrophobic material is insufficient in bonding strength between the hydrophobic layer and the negative electrode material layer, insufficient hardness of the hydrophobic layer, and looseness of the hydrophobic layer and easy falling off and damage are solved. The invention solves the problem of the hydrophobic layer falling off and being damaged from the negative electrode material layer, and reduces the negative influence of the hydrophobic layer on the electrochemical interface reaction of the aqueous nickel-zinc secondary battery; the negative electrode material layer of the negative electrode plate is coated with the hydrophobic layer, and the contact between the active material of the negative electrode material layer and the electrolyte is blocked by the hydrophobic layer, and a hydrophobic layer is constructed on the surface of the negative electrode plate to block the contact between the active material zinc of the negative electrode plate and the alkaline electrolyte, which can effectively reduce or even avoid the chemical reaction between the active material zinc and the alkaline electrolyte, effectively reduce or even avoid the zinc dendrites of the aqueous nickel-zinc secondary battery and the passivation of the surface of the negative electrode plate, solves the problem of continuous corrosion and hydrogen evolution of the aqueous nickel-zinc secondary battery during storage and circulation, which causes the battery shell to swell and bulge and even leak, can effectively reduce or even avoid the corrosion and hydrogen evolution of the active material of the negative electrode plate, take into account the long storage performance and cycle life performance of the aqueous nickel-zinc secondary battery, and significantly improve the cycle life performance of the aqueous nickel-zinc secondary battery.

[0016] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The above and other objects, features and advantages of the present application will become more apparent by describing in more detail exemplary embodiments of the present application in conjunction with the accompanying drawings, wherein the same reference numerals generally represent the same components in the exemplary embodiments of the present application.

[0018] Figure 1 It is a schematic cross-sectional view of the negative electrode sheet of an aqueous nickel-zinc secondary battery shown in an embodiment of the present application. DETAILED DESCRIPTION

[0019] The embodiments of the present application will be described in more detail below with reference to the accompanying drawings. Although the embodiments of the present application are shown in the accompanying drawings, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to make the present application more thorough and complete, and to fully convey the scope of the present application to those skilled in the art.

[0020] The terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The singular forms of "a", "said" and "the" used in this application and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0021] It should be understood that although the terms "first", "second", "third", etc. may be used in this application to describe various information, this information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of this application, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0022] The embodiment of the present application provides a negative electrode plate for an aqueous nickel-zinc secondary battery, which can effectively reduce or even avoid the corrosion and hydrogen evolution of the active material of the negative electrode plate, take into account the long storage performance and cycle life performance of the aqueous nickel-zinc secondary battery, and significantly improve the cycle life performance of the aqueous nickel-zinc secondary battery.

[0023] The technical solution of the embodiments of the present application is described in detail below with reference to the accompanying drawings.

[0024] Figure 1 It is a schematic cross-sectional view of the negative electrode sheet of an aqueous nickel-zinc secondary battery shown in an embodiment of the present application.

[0025] See also Figure 1 A negative electrode plate for an aqueous nickel-zinc secondary battery comprises a current collector 103, a negative electrode material layer 101 disposed on at least one side of the current collector 103, and a hydrophobic layer 102 coating the negative electrode material layer 101, wherein the hydrophobic layer 102 is used to isolate the contact between the negative electrode material layer 101 and an electrolyte; wherein the hydrophobic layer 102 comprises a hydrophobic material, the hydrophobic material comprises a first type of hydrophobic material and a second type of hydrophobic material, the particle size of the first type of hydrophobic material is smaller than the particle size of the second type of hydrophobic material, and the first type of hydrophobic material comprises polyetheretherketone.

[0026] In one embodiment, the negative electrode slurry of the aqueous nickel-zinc secondary battery can be coated on the negative electrode collector, and then dried, rolled, softened, and cut to obtain a negative electrode plate of a suitable size; the hydrophobic material including the first hydrophobic material polyetheretherketone and the second hydrophobic material is evenly mixed with a solvent to prepare a hydrophobic liquid for the hydrophobic layer, wherein the small-particle first hydrophobic material polyetheretherketone is doped in the large-particle second hydrophobic material, and the small-particle first hydrophobic material polyetheretherketone can fill the pores of the large-particle second hydrophobic material; the hydrophobic liquid is sprayed on the surface of the negative electrode material layer of the negative electrode plate of a suitable size; the negative electrode plate sprayed with the hydrophobic liquid is dried and rolled to obtain a negative electrode plate in which the negative electrode material layer is coated with the hydrophobic layer, and the contact between the negative electrode material layer and the electrolyte is blocked by the hydrophobic layer.

[0027] The negative electrode plate of the aqueous nickel-zinc secondary battery of the embodiment of the present application includes a current collector, a negative electrode material layer arranged on at least one side of the current collector, and a hydrophobic layer coating the negative electrode material layer, the hydrophobic layer is used to isolate the contact between the negative electrode material layer and the electrolyte; wherein the hydrophobic layer includes a hydrophobic material, the hydrophobic material includes a first type of hydrophobic material and a second type of hydrophobic material, the particle size of the first type of hydrophobic material is smaller than the particle size of the second type of hydrophobic material, the first type of hydrophobic material includes polyetheretherketone, and the bonding strength and hydrophobicity of the hydrophobic layer can be improved by doping the first type of hydrophobic material polyetheretherketone with a small particle size with the second type of hydrophobic material with a large particle size, so that the hydrophobic layer has stronger hydrophobicity and better bonding, and the bonding strength between the hydrophobic layer and the negative electrode material layer is improved. By including the hydrophobic layer of the first type of hydrophobic material polyetheretherketone and the second type of hydrophobic material, the problems of insufficient bonding strength between the hydrophobic layer and the negative electrode material layer, insufficient hardness of the hydrophobic layer, and looseness and easy falling off and damage of the hydrophobic layer are solved. The negative electrode material layer of the negative electrode plate is coated with the hydrophobic layer, and the contact between the active material of the negative electrode material layer and the electrolyte is blocked by the hydrophobic layer. A hydrophobic layer is constructed on the surface of the negative electrode plate to block the contact between the active material zinc of the negative electrode plate and the alkaline electrolyte, which can effectively reduce or even avoid the chemical reaction between the active material zinc and the alkaline electrolyte, effectively reduce or even avoid the zinc dendrites of the aqueous nickel-zinc secondary battery and the passivation of the surface of the negative electrode plate, solve the problem of continuous corrosion and hydrogen evolution of the aqueous nickel-zinc secondary battery during storage and circulation, causing the battery shell to swell and grow high or even leak, can effectively reduce or even avoid the corrosion and hydrogen evolution of the active material of the negative electrode plate, take into account the long storage performance and cycle life performance of the aqueous nickel-zinc secondary battery, and significantly improve the cycle life performance of the aqueous nickel-zinc secondary battery.

[0028] In one embodiment, a negative electrode plate of an aqueous nickel-zinc secondary battery includes a current collector, a negative electrode material layer, and a hydrophobic layer arranged in sequence; wherein the negative electrode material layer is disposed on at least one side of the current collector, the hydrophobic layer covers the negative electrode material layer, and the hydrophobic layer is used to isolate the contact between the negative electrode material layer and the electrolyte.

[0029] In one embodiment, each component of the negative electrode material can be weighed according to the mass percentage of the negative electrode material, an appropriate amount of pure water is added to the negative electrode material, and the negative electrode material is stirred evenly to prepare a negative electrode slurry; the negative electrode slurry is applied to a current collector (for example, a copper-plated tinned inclined wire mesh substrate) by a paste coating method, and the negative electrode slurry and the current collector are compounded, and then dried, rolled, softened, and cut to obtain a negative electrode sheet with a negative electrode material layer of a suitable size; the negative electrode material layer of the negative electrode sheet of a suitable size is coated with a hydrophobic layer to isolate the contact between the active material of the negative electrode material layer and the electrolyte, thereby obtaining a negative electrode sheet of an aqueous nickel-zinc secondary battery.

[0030] In one embodiment, a hydrophobic layer can be prepared by using a hydrophobic material, and the negative electrode material layer of the negative electrode plate of a suitable size is coated by the hydrophobic layer to cut off the contact between the active material of the negative electrode material layer and the electrolyte. The hydrophobic material of the hydrophobic layer includes a first type of hydrophobic material and a second type of hydrophobic material. The particle size of the first type of hydrophobic material is smaller than that of the second type of hydrophobic material. The first type of hydrophobic material includes polyetheretherketone (Poly(Ether-Ether-Ketone) PEEK), and the second type of hydrophobic material includes PMMA (Polymethyl Methacrylate) and / or fluoroplastics.

[0031] In one embodiment, the fluoroplastic includes one or more of PTFE (Polytetrafluoroethylene), FEP (Fluorinated Ethylene Propylene), ETFE (Ethylene-Tetra-Fluoro-Ethylene), and PFA (Fluoroplastic).

[0032] In one embodiment, the particle size of the first type of hydrophobic material is less than half of the particle size of the second type of hydrophobic material.

[0033] In one embodiment, a hydrophobic liquid can be prepared by mixing a hydrophobic material with a set solvent in a set mass ratio, and the hydrophobic liquid is sprayed on the negative electrode material layer in a set spraying amount. After drying and rolling, a hydrophobic layer is formed on the surface of the negative electrode material layer; the negative electrode material layer of a negative electrode sheet of a suitable size is coated with the hydrophobic layer to isolate the active material of the negative electrode material layer from contact with the electrolyte.

[0034] In one embodiment, the mass ratio of the hydrophobic material to the set solvent is (1:19)-(1:10). The hydrophobic material and the set solvent of the set mass ratio can be mixed evenly according to the mass ratio of the hydrophobic material to the set solvent to form a hydrophobic liquid; the hydrophobic liquid is sprayed on the surface of the negative electrode material layer on both sides of the current collector of the negative electrode plate of suitable size by a spraying device according to a set spraying amount; the negative electrode plate sprayed with the hydrophobic liquid is dried, and the dried negative electrode plate is rolled under a set pressure to obtain a negative electrode plate of an aqueous nickel-zinc secondary battery, wherein the negative electrode plate has a hydrophobic layer covering the negative electrode material layer.

[0035] In one embodiment, in 100 grams of hydrophobic material, the ratio of the mass percentage of the first type of hydrophobic material to the mass percentage of the second type of hydrophobic material is in the range of (20%:80%) to (40%:60%).

[0036] In one embodiment, the first type of hydrophobic material is polyetheretherketone, and the second type of hydrophobic material is polytetrafluoroethylene; wherein in 100 grams of hydrophobic material, the mass percentage of polyetheretherketone to the mass percentage of polytetrafluoroethylene ranges from (20%:80%) to (40%:60%).

[0037] In one embodiment, the solvent is set to be ethanol; wherein the mass ratio of the mass of polyetheretherketone and polytetrafluoroethylene to the mass of ethanol is (1:19)-(1:10).

[0038] In one embodiment, the particle size of polyetheretherketone is 2 μm-5 μm, and the particle size of polytetrafluoroethylene is 20 μm-30 μm.

[0039] In one embodiment, the first type of hydrophobic material is PEEK, and the second type of hydrophobic material is PTFE. In 100 grams of hydrophobic material, the mass percentage of PEEK and the mass percentage of PTFE are in a ratio of 40%:60%. PEEK and PTFE in a mass percentage ratio of 40%:60% are evenly mixed in a set solvent ethanol to form a hydrophobic liquid, wherein the mass ratio of PEEK and PTFE to the mass of the set solvent ethanol is (1:19)-(1:10); the hydrophobic liquid is sprayed on the surface of the negative electrode material layer on both sides of the negative electrode plate current collector of a suitable size by a spraying device according to a set spraying amount; the negative electrode plate sprayed with the hydrophobic liquid is dried, and the dried negative electrode plate is rolled under a set pressure to obtain a negative electrode plate of an aqueous nickel-zinc secondary battery, wherein the negative electrode plate has a hydrophobic layer of mixed PEEK and PTFE covering the negative electrode material layer.

[0040] In one embodiment, the hydrophobic layer coating the negative electrode material layer is a mixture of PEEK and PTFE, which not only makes the hydrophobic layer have good hydrophobic properties and can isolate the contact between the negative electrode material layer and the electrolyte, but also the PEEK with small particle size can be fully filled in the pores of PTFE, so that the hydrophobic layer has good hydrophobicity, wear resistance and adhesion, so that the hydrophobic layer can firmly adhere to the surface of the negative electrode material layer, making it difficult for the hydrophobic layer to fall off and be damaged during the manufacturing and use of the battery, thereby avoiding the incompleteness of the hydrophobic layer caused by the shedding and damage of the hydrophobic layer, which in turn aggravates the corrosion of the negative electrode material layer in the area where the hydrophobic layer is missing.

[0041] In one embodiment, the set spraying amount of the hydrophobic liquid is 5g / m 2 -15g / m 2 The hydrophobic liquid can be prepared by mixing a 40%:60% PEEK and PTFE mixed solid powder with a set solvent ethanol at a mass ratio of 1:19-1:10; the spraying amount is 5g / m 2 -15g / m 2 , spraying a hydrophobic liquid on the surface of the negative electrode material layer on both sides of the current collector of a negative electrode plate of suitable size; placing the negative electrode plate sprayed with the hydrophobic liquid in an oven to completely evaporate the set solvent ethanol and dry it; rolling the dried negative electrode plate under a set pressure to firmly combine the hydrophobic layer of mixed PEEK and PTFE on the surface of the negative electrode material layer with the negative electrode material layer, thereby obtaining a negative electrode plate of an aqueous nickel-zinc secondary battery with a strong corrosion-resistant hydrogen evolution hydrophobic layer, wherein the hydrophobic layer of mixed PEEK and PTFE covers the negative electrode material layer of the negative electrode plate.

[0042] In one embodiment, the preferred spraying amount of the hydrophobic liquid is 5 g / m 2 -10g / m 2 .

[0043] In one embodiment, the ethanol may be an ethanol solution with a concentration of 99.7%, for example, industrial alcohol.

[0044] In one embodiment, the pressure of the roller pressing is 1Mpa (megapascal) to 5Mpa. If the pressure of the roller pressing is too small, the negative electrode sheet cannot be compacted, and the hydrophobic layer and the negative electrode material layer cannot be tightly combined. If the pressure of the roller pressing is too large, the hydrophobic layer may rupture and fall off, and the contact between the negative electrode material layer and the electrolyte cannot be cut off.

[0045] In one embodiment, the greater the mass ratio of the mixed solid powder of the hydrophobic material including the first type of hydrophobic material and the second type of hydrophobic material to the set solvent ethanol and / or the greater the spraying amount, the thicker the hydrophobic layer will be, the better the hydrophobic effect will be, and the better the effect of isolating the active material of the negative electrode material layer from contact with the electrolyte will be, but an excessively thick hydrophobic coating will affect the electron transfer rate of the negative electrode.

[0046] In one embodiment, the negative electrode material layer of the negative electrode plate includes 50%wt-65%wt of spherical ZnO (zinc oxide) powder, 5%wt-10%wt of Zn (zinc) nanopowder, 0.05%wt-0.1%wt of Bi2O3 (bismuth trioxide), 0.01%wt-0.05%wt of In2O3 (indium trioxide), 0.01%wt-0.05%wt of anionic surfactant, 1 wt%-5wt% of conductive carbon powder, and 20%wt-25%wt of binder. In the negative electrode material layer of the embodiment of the present application, bismuth oxide and indium oxide have a higher hydrogen evolution potential, which can inhibit the formation of zinc dendrites of the negative electrode material and inhibit the corrosion of active substances; the conductive carbon powder can enhance the conductivity of the plate and enhance the negative electrode rate discharge performance; the anionic surfactant can inhibit the corrosion of negative zinc and the generation of zinc dendrites.

[0047] In one embodiment, the anionic surfactant may be sodium dodecylbenzene sulfonate and / or sodium dodecylbenzene sulfonate.

[0048] In one embodiment, the binder includes one or more of carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), and PTFE.

[0049] In one embodiment, during the preparation of the negative electrode slurry, a binder solid powder may be added to pure water, and a binder aqueous solution with a set mass percentage may be prepared by mechanical stirring; the binder aqueous solution and other materials of the negative electrode material may be stirred evenly to prepare the negative electrode slurry. For example, a CMC aqueous solution with a CMC mass percentage of 2% may be stirred evenly with other materials of the negative electrode material to prepare the negative electrode slurry; wherein, a CMC aqueous solution with a CMC mass percentage of 2% refers to a solution containing 2 grams of CMC solid powder in 100 grams of CMC aqueous solution.

[0050] The negative electrode plate of the aqueous nickel-zinc secondary battery of the embodiment of the present application comprises a current collector, a negative electrode material layer arranged on at least one side of the current collector, and a hydrophobic layer coating the negative electrode material layer, wherein the hydrophobic layer is used to isolate the contact between the negative electrode material layer and the electrolyte; wherein the hydrophobic layer comprises a hydrophobic material, the hydrophobic material comprises a first type of hydrophobic material and a second type of hydrophobic material, the particle size of the first type of hydrophobic material is smaller than the particle size of the second type of hydrophobic material, the first type of hydrophobic material comprises polyetheretherketone, by doping the first type of hydrophobic material polyetheretherketone with a large particle size of the second type of hydrophobic material, the bonding strength and hydrophobicity of the hydrophobic layer can be improved, so that the hydrophobic layer has stronger hydrophobicity and better bonding, and the bonding strength between the hydrophobic layer and the negative electrode material layer is improved, and the hydrophobic layer comprising the first type of hydrophobic material polyetheretherketone and the second type of hydrophobic material is used to solve the problems of insufficient bonding strength between the hydrophobic layer and the negative electrode material layer, insufficient hardness of the hydrophobic layer, looseness of the hydrophobic layer, and easy falling off and damage of the hydrophobic layer, and avoid the hydrophobic layer from the negative electrode material The material layer falls off and is damaged, reducing the negative impact of the hydrophobic layer on the electrochemical interface reaction of the aqueous nickel-zinc secondary battery; the negative electrode material layer of the negative electrode plate is coated with the hydrophobic layer, and the contact between the active material of the negative electrode material layer and the electrolyte is blocked by the hydrophobic layer, and a hydrophobic layer is constructed on the surface of the negative electrode plate to block the contact between the active material zinc of the negative electrode plate and the alkaline electrolyte, which can effectively slow down or even avoid the dissolution and shedding of the active material and the hydrogen evolution reaction, effectively reduce or even avoid the chemical reaction between the active material zinc and the alkaline electrolyte, effectively reduce or even avoid the zinc dendrites of the aqueous nickel-zinc secondary battery and the passivation of the surface of the negative electrode plate, solve the problem of uninterrupted corrosion and hydrogen evolution of the aqueous nickel-zinc secondary battery during storage and circulation, causing the battery shell to swell and grow high or even leak, can effectively reduce or even avoid the corrosion and hydrogen evolution of the active material of the negative electrode plate, take into account the long storage performance and cycle life performance of the aqueous nickel-zinc secondary battery, and significantly improve the cycle life performance of the aqueous nickel-zinc secondary battery.

[0051] Furthermore, in the negative electrode plate of the aqueous nickel-zinc secondary battery of the embodiment of the present application, the negative electrode material layer of the negative electrode plate is coated with a hydrophobic layer, and the hydrophobic layer is used to isolate the contact between the active material of the negative electrode material layer and the electrolyte. The hydrophobic material of the hydrophobic layer is polyetheretherketone and polytetrafluoroethylene. The hydrophobic material of the hydrophobic layer has low cost and excellent performance, is safe and environmentally friendly, and will not significantly increase the manufacturing cost and environmental cost of the aqueous nickel-zinc secondary battery.

[0052] In addition, an embodiment of the present application further provides an aqueous nickel-zinc secondary battery, which includes a positive electrode plate, an electrolyte, a separator, and the above-mentioned negative electrode plate.

[0053] In one embodiment, the positive electrode plate of the aqueous nickel-zinc secondary battery includes a positive electrode current collector and a positive electrode material coated on the positive electrode current collector; wherein the positive electrode slurry of the positive electrode material includes 70%wt-75%wt of spherical β-Ni(OH)2 (nickel hydroxide) with a surface coated with trivalent cobalt, 0.01%wt-0.05%wt of Ca(OH)2 (calcium hydroxide), 3%wt-4%wt of a conductive agent, 0.5%wt-1%wt of Y2O3 (yttrium trioxide) or 0.5%wt-1%wt of Yb2O3 (ytterbium trioxide), 2%wt-3%wt of a binder, 1%wt-2%wt of a suspending agent, and the remainder is pure water.

[0054] In one embodiment, the conductive agent can be selected from one or more of Cu (copper), Ni (nickel), and Zn (zinc). In a specific embodiment, the conductive agent has a particle size of 1 μm (micrometer) to 3 μm and a tap density of 1 g / cm 3 (grams per cubic centimeter) - 3g / cm 3 Ni powder.

[0055] In a specific embodiment, the binder having a dispersing and bonding effect can be prepared by first preparing a binder aqueous solution when preparing the positive electrode slurry; then the binder aqueous solution and other materials of the positive electrode material are stirred evenly to prepare the positive electrode slurry. In a specific embodiment, the binder aqueous solution can be a CMC aqueous solution and / or a PTFE aqueous solution. The CMC aqueous solution can be a CMC aqueous solution with a CMC mass percentage of 2%. The PTFE aqueous solution can be a PTFE aqueous solution with a PTFE mass percentage of 60%. In a specific embodiment, a polytetrafluoroethylene solid powder and pure water with a mass ratio of 3:2 can be fully stirred evenly by a magnetic stirrer to obtain a 60%wt PTFE aqueous solution.

[0056] In a specific embodiment, the spherical β-Ni(OH)2 with trivalent cobalt on the surface of the active material and the conductive nickel powder have relatively high density. When the positive electrode slurry is left standing, the high-density substances will sink to the bottom. Adding the suspending agent xanthan gum to the positive electrode slurry can avoid the sinking of high-density substances when the positive electrode slurry is left standing.

[0057] In a specific embodiment, the positive electrode material can be mixed with an appropriate amount of pure water to prepare a positive electrode slurry; the positive electrode slurry is applied to a surface density of 250g / m 2 (grams per square meter)-380g / m 2 The positive electrode current collector (for example, nickel foam) is prepared, and the positive electrode slurry is compounded with the positive electrode current collector to obtain a positive electrode sheet of an aqueous nickel-zinc secondary battery.

[0058] In one embodiment, the electrolyte of the aqueous nickel-zinc secondary battery may be one or more of KOH (potassium hydroxide), NaOH (sodium hydroxide), LiOH (lithium hydroxide), Al(OH)3 (aluminum hydroxide), and Zn(OH)2 (zinc hydroxide).

[0059] In one embodiment, the electrolyte further includes 0.03 mol / L-0.5 mol / L ZnO to inhibit the dissolution of the negative electrode material layer in the electrolyte.

[0060] In one embodiment, the electrolyte further includes a buffer, and the buffer may be phosphate.

[0061] In one embodiment, the pH value of the electrolyte is 10-14 at 25 degrees Celsius, and the conductivity is 350 mS / cm (milliSiemens per centimeter)-470 mS / cm. In order to improve the cycle performance of the aqueous nickel-zinc secondary battery of the embodiment of the present application, the amount of electrolyte injected is 1 / 5 of the weight of the positive electrode sheet and the negative electrode sheet.

[0062] In one embodiment, the diaphragm of the aqueous nickel-zinc secondary battery can absorb alkali solution and insulate to prevent short circuit, and adopts a dendrite-proof composite diaphragm of one layer of non-woven fabric and three layers of PE (Polyethylene), or a dendrite-proof composite diaphragm of one layer of non-woven fabric and three layers of PP. The alkali-absorbing non-woven fabric facing the positive electrode plate is hydrophilized by sulfonation or grafting, and the three-layer PE microporous diaphragm or three-layer PP microporous diaphragm facing the negative electrode plate is hydrophilized by sulfonation or grafting.

[0063] The negative electrode sheet of the aqueous nickel-zinc secondary battery of the embodiment of the present application is described below with reference to Examples 1-13 and Comparative Examples.

[0064] According to the design of 2A1500 battery cells, the positive electrode sheets and negative electrode sheets of Examples 1-13 and the comparative example are cut to obtain the positive electrode sheets and negative electrode sheets of appropriate sizes.

[0065] Comparative Example: In the comparative example, the negative electrode plate is not coated with the hydrophobic layer of the negative electrode material layer, and the set spraying amount of the hydrophobic liquid is 0.

[0066] Embodiment 1: In Example 1, the hydrophobic material of the hydrophobic layer coating the negative electrode material layer of the negative electrode plate is a mixed solid powder of PEEK and PTFE, wherein in 100 grams of the mixed solid powder of PEEK and PTFE, the mass percentage of PEEK to the mass percentage of PTFE is 40%:60%; the mass ratio of the mixed solid powder of PEEK and PTFE to ethanol is 1:19 to prepare a hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 2 g / m 2 .

[0067] Embodiment 2: In Example 2, the hydrophobic material of the hydrophobic layer coating the negative electrode material layer of the negative electrode plate is a mixed solid powder of PEEK and PTFE, wherein in 100 grams of the mixed solid powder of PEEK and PTFE, the mass percentage of PEEK to the mass percentage of PTFE is 40%:60%; the mass ratio of the mixed solid powder of PEEK and PTFE to ethanol is 1:19 to prepare a hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 5g / m 2 .

[0068] Embodiment 3: In Example 3, the hydrophobic material of the hydrophobic layer coating the negative electrode material layer of the negative electrode plate is a mixed solid powder of PEEK and PTFE, wherein in 100 grams of the mixed solid powder of PEEK and PTFE, the mass percentage of PEEK to the mass percentage of PTFE is 40%:60%; the mass ratio of the mixed solid powder of PEEK and PTFE to ethanol is 1:19 to prepare a hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 8 g / m 2 .

[0069] Embodiment 4: In Example 4, the hydrophobic material of the hydrophobic layer coating the negative electrode material layer of the negative electrode plate is a mixed solid powder of PEEK and PTFE, wherein in 100 grams of the mixed solid powder of PEEK and PTFE, the mass percentage of PEEK to the mass percentage of PTFE is 40%:60%; the mass ratio of the mixed solid powder of PEEK and PTFE to ethanol is 1:19 to prepare a hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 10g / m 2 .

[0070] Embodiment 5: In Example 5, the hydrophobic material of the hydrophobic layer coating the negative electrode material layer of the negative electrode plate is a mixed solid powder of PEEK and PTFE, wherein in 100 grams of the mixed solid powder of PEEK and PTFE, the mass percentage of PEEK to the mass percentage of PTFE is 40%:60%; the mass ratio of the mixed solid powder of PEEK and PTFE to ethanol is 1:19 to prepare a hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 12 g / m 2 .

[0071] Embodiment 6: In Example 6, the hydrophobic material of the hydrophobic layer coating the negative electrode material layer of the negative electrode plate is a mixed solid powder of PEEK and PTFE, wherein in 100 grams of the mixed solid powder of PEEK and PTFE, the mass percentage of PEEK to the mass percentage of PTFE is 40%:60%; the mass ratio of the mixed solid powder of PEEK and PTFE to ethanol is 1:19 to prepare a hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 15 g / m 2 .

[0072] Embodiment 7: In Example 7, the hydrophobic material of the hydrophobic layer coating the negative electrode material layer of the negative electrode plate is a mixed solid powder of PEEK and PTFE, wherein in 100 grams of the mixed solid powder of PEEK and PTFE, the mass percentage of PEEK to the mass percentage of PTFE is 40%:60%; the mass ratio of the mixed solid powder of PEEK and PTFE to ethanol is 1:19 to prepare a hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 20 g / m 2 .

[0073] Embodiment 8: In Example 8, the hydrophobic material of the hydrophobic layer coating the negative electrode material layer of the negative electrode plate is a mixed solid powder of PEEK and PMMA, wherein in 100 g of the mixed solid powder of PEEK and PMMA, the mass percentage of PEEK to the mass percentage of PMMA is 40%:60%; the mass ratio of the mixed solid powder of PEEK and PMMA to ethanol is 1:19 to prepare a hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 10 g / m 2 .

[0074] Embodiment 9: In Example 9, the hydrophobic material of the hydrophobic layer covering the negative electrode material layer of the negative electrode plate is PTFE solid powder, the mass ratio of PTFE mixed solid powder to ethanol is 1:19 to prepare hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 10g / m 2 .

[0075] Embodiment 10: In Example 10, the hydrophobic material of the hydrophobic layer coating the negative electrode material layer of the negative electrode plate is PEEK and PTFE solid powder, wherein in 100 grams of PEEK and PTFE mixed solid powder, the mass percentage of PEEK to the mass percentage of PTFE is 20%:80%; the mass ratio of the PEEK and PTFE mixed solid powder to ethanol is 1:19 to prepare a hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 10g / m 2 .

[0076] Embodiment 11: In Example 11, the hydrophobic material of the hydrophobic layer coating the negative electrode material layer of the negative electrode plate is PEEK and PTFE solid powder, wherein in 100 grams of PEEK and PTFE mixed solid powder, the mass percentage of PEEK to the mass percentage of PTFE is 60%:40%; the mass ratio of the PEEK and PTFE mixed solid powder to ethanol is 1:19 to prepare a hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 10g / m 2 .

[0077] Embodiment 12: In Example 12, the hydrophobic material of the hydrophobic layer coating the negative electrode material layer of the negative electrode plate is PEEK and PTFE solid powder, wherein in 100 grams of PEEK and PTFE mixed solid powder, the mass percentage of PEEK to the mass percentage of PTFE is 80%:20%; the mass ratio of the PEEK and PTFE mixed solid powder to ethanol is 1:19 to prepare a hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 10g / m 2 .

[0078] Embodiment 13: In Example 13, the hydrophobic material of the hydrophobic layer coating the negative electrode material layer of the negative electrode plate is PEEK solid powder, and the mass ratio of PEEK solid powder to ethanol is 1:19 to prepare a hydrophobic liquid, and the set spraying amount of the hydrophobic liquid is 10g / m 2 .

[0079] The positive electrode sheet is wrapped around the negative electrode sheet, and the positive electrode sheet, negative electrode sheet and separator of Examples 1-13 and the comparative example are wound to obtain the battery cells corresponding to Examples 1-13 and the comparative example; wherein, the positive electrode is connected to the positive electrode cap, and the negative electrode is in contact with the steel shell. The positive electrode ear is made of pure nickel. In order to prevent the zinc in the negative electrode sheet from forming a micro-battery with the iron element in the steel shell to produce side reactions, a layer of tin-plated copper foil slightly wider than the negative electrode sheet, with a total thickness of 0.03 mm (millimeter) and a tin-plated layer thickness of 5 μm is wrapped around the outermost side of the battery electrode group.

[0080] The prepared electrolyte was injected according to the total mass of the positive electrode sheet and the negative electrode sheet to prepare aqueous nickel-zinc secondary batteries corresponding to Examples 1-13 and the comparative example, respectively.

[0081] After the aqueous nickel-zinc secondary batteries corresponding to Examples 1-13 and the comparative examples were manufactured, the actual capacities were confirmed through formation. According to the actual capacities, the aqueous nickel-zinc secondary batteries corresponding to Examples 1-13 and the comparative examples were subjected to accelerated tests of 80°C (degrees Celsius) high temperature storage test and 1C charge-discharge cycle test, and the 5-day SOC, 10-day SOC, 15-day SOC, and 150cyc-SOH of the aqueous nickel-zinc secondary batteries corresponding to Examples 1-13 and the comparative examples were obtained, respectively, as shown in Tables 1 to 4.

[0082] The 80℃ high-temperature storage test is to place the fully charged battery in an 80℃ constant temperature oven, take out three batteries every 5 days, and discharge them after the batteries have cooled to the room temperature of 25℃. The discharge amount is divided by the actual capacity before placement and recorded as SOC. The SOC of the three batteries is then averaged. The 1C charge and discharge is based on the actual capacity of the battery. For example, if the actual capacity of the battery is 1460mAh, the charge and discharge are both set to 1460mAh cutoff.

[0083] 150cyc-SOH indicates the battery health status after 150 cycles. SOH (State Of Health) is a numerical value indicating the battery health status.

[0084] SOC (State of Charge) is used to reflect the remaining capacity of the battery. Its value is defined as the ratio of the remaining capacity to the battery capacity. It is usually expressed as a percentage and its value range is 0% to 100%. When SOC = 0%, it means the battery is fully discharged, and when SOC = 100%, it means the battery is fully charged.

[0085] Table 1:

[0086] Table 2

[0087] Table 3

[0088] Table 4

[0089] According to the comparative examples in Table 1 and Table 2, Examples 1-9, and Example 13, the 150cyc-SOH of the aqueous nickel-zinc secondary battery corresponding to Examples 4 and 8, in which a hydrophobic liquid of a mixture of PEEK and PTFE or a mixture of PEEK and PMMA is sprayed on the negative electrode plate, and the negative electrode material layer of the negative electrode plate is coated with a hydrophobic layer of a mixture of PEEK and PTFE or a mixture of PEEK and PMMA, is significantly better than the 150cyc-SOH of the aqueous nickel-zinc secondary battery corresponding to Examples 9 and 13 of a single hydrophobic material, and increases significantly with the increase in the amount of the hydrophobic liquid sprayed with the mixed PEEK and PTFE, thereby significantly improving the 150cyc-SOH of the aqueous nickel-zinc secondary battery. The mixed first hydrophobic material PEEK and the second hydrophobic material of the negative electrode plate of the nickel-zinc secondary battery are mixed with the second hydrophobic material with a large particle size by the small particle size of the first hydrophobic material polyetheretherketone, which can improve the bonding strength and hydrophobicity of the hydrophobic layer, make the hydrophobic layer more hydrophobic and have better bonding, and improve the bonding strength between the hydrophobic layer and the negative electrode material layer. The hydrophobic layer including the first hydrophobic material polyetheretherketone and the second hydrophobic material solves the problems of insufficient bonding strength between the hydrophobic layer and the negative electrode material layer, insufficient hardness of the hydrophobic layer, looseness of the hydrophobic layer, and easy falling off and damage, avoids the hydrophobic layer from falling off and damage from the negative electrode material layer, and reduces the negative influence of the hydrophobic layer on the electrochemical interface reaction of the aqueous nickel-zinc secondary battery; the hydrophobic layer can significantly improve the cycle life performance of the aqueous nickel-zinc secondary battery.

[0090] According to the comparative examples in Table 1 and Table 2, and the 5-day-SOC, 10-day-SOC, and 15-day-SOC of the aqueous nickel-zinc secondary battery corresponding to Examples 1-7, the SOC gradually deteriorates with the increase in the amount of the mixed PEEK and PTFE hydrophobic liquid sprayed, and the deterioration trend becomes more serious with the increase in the amount of the mixed hydrophobic liquid sprayed. The hydrophobic liquid of the mixed PEEK and PTFE is sprayed on the negative electrode plate, and the negative electrode material layer of the negative electrode plate is coated with a hydrophobic layer of the mixed PEEK and PTFE. Although the contact between the active material of the negative electrode material layer and the electrolyte is cut off, the problem of continuous corrosion and hydrogen evolution of the aqueous nickel-zinc secondary battery during storage and circulation, and the corrosion and hydrogen evolution causing the battery shell to expand and bulge, grow high, and even leak, is solved. However, the contact between the active material of the negative electrode material layer and the electrolyte is cut off, and the electrolyte is more distributed to the positive electrode plate, resulting in the expansion, fragmentation, and cracking of the active material of the positive electrode plate, and the conductive cobalt coating layer on its surface also falls off with the peeling, which deteriorates the high-temperature storage performance of the aqueous nickel-zinc secondary battery.

[0091] However, according to the comparative examples in Table 1 and Table 2, and the 150cyc-SOH of the corresponding aqueous nickel-zinc secondary batteries of Examples 1-7, a hydrophobic liquid of a mixture of PEEK and PTFE is sprayed on the negative electrode plate, and the negative electrode material layer of the negative electrode plate is coated with a hydrophobic layer of a mixture of PEEK and PTFE. The 150cyc-SOH of the aqueous nickel-zinc secondary batteries corresponding to Examples 1-7 significantly increases with the increase in the spraying amount of the mixed PEEK and PTFE hydrophobic liquid, thereby significantly improving the 150cyc-SOH of the aqueous nickel-zinc secondary batteries. It can be seen that the mixed PEEK and PTFE hydrophobic layer of the negative electrode plate of the aqueous nickel-zinc secondary battery slows down the dissolution and shedding of the active material of the negative electrode plate and the hydrogen evolution reaction, and effectively improves the cycle life of the aqueous nickel-zinc secondary battery; the negative electrode material layer of the negative electrode plate is coated with a mixed PEEK and PTFE hydrophobic layer to isolate the contact between the active material of the negative electrode material layer and the electrolyte, and a hydrophobic layer is constructed on the surface of the negative electrode plate to isolate the contact between the active material zinc of the negative electrode plate and the alkaline electrolyte, which can effectively reduce or even avoid the chemical reaction between the active material zinc and the alkaline electrolyte, effectively reduce or even avoid the zinc dendrites of the aqueous nickel-zinc secondary battery and the passivation of the surface of the negative electrode plate, can effectively reduce or even avoid the corrosion and hydrogen evolution of the active material of the negative electrode plate, can take into account the long storage performance and cycle life performance of the aqueous nickel-zinc secondary battery, and the mixed PEEK and PTFE hydrophobic layer of the negative electrode plate of the aqueous nickel-zinc secondary battery can significantly improve the cycle life performance of the aqueous nickel-zinc secondary battery.

[0092] According to the 150cyc-SOH of the aqueous nickel-zinc secondary battery corresponding to Examples 1-7 in Table 1 and Table 2, a hydrophobic liquid mixed with PEEK and PTFE is sprayed on the negative electrode plate. When the spraying amount of the hydrophobic liquid is greater than or equal to 20g / m 2When the negative electrode is completely hydrophobic, a hydrophobic layer is formed on the surface of the negative electrode plate, making the negative electrode plate completely hydrophobic, completely isolating the contact between the negative electrode plate and the alkaline electrolyte, increasing the proportion of the electrolyte in the positive electrode plate, aggravating the corrosion and expansion of the positive electrode active material, and reducing the cycle life of the corresponding aqueous nickel-zinc secondary battery. Therefore, the mass ratio of the mixed solid powder of the hydrophobic material in the hydrophobic liquid to the set solvent ethanol, as well as the spraying amount of the hydrophobic liquid should be comprehensively considered to form a suitable hydrophobic layer of mixed PEEK and PTFE on the negative electrode material layer, so as to take into account the long storage performance and cycle life performance of the aqueous nickel-zinc secondary battery, and significantly improve the cycle life performance of the aqueous nickel-zinc secondary battery.

[0093] According to the data of Example 4 in Table 3 and Example 8 in Table 4, the 5-day-SOC, 10-day-SOC, 15-day-SOC and 150cyc-SOH of the aqueous nickel-zinc secondary battery corresponding to Example 4 in which the second hydrophobic material is PTFE are better than the 5-day-SOC, 10-day-SOC, 15-day-SOC and 150cyc-SOH of the aqueous nickel-zinc secondary battery corresponding to Example 8 in which the second hydrophobic material is PMMA. The high-temperature storage performance and cycle life performance of the aqueous nickel-zinc secondary battery corresponding to Example 4 in which the second hydrophobic material is PTFE are better than the high-temperature storage performance and cycle life performance of the aqueous nickel-zinc secondary battery corresponding to Example 8 in which the second hydrophobic material is PMMA. The hydrophobic liquid mixed with the second hydrophobic material PMMA in Example 8 can form a dense hydrophobic layer on the negative electrode material layer, and the negative electrode interface reaction of the aqueous nickel-zinc secondary battery corresponding to Example 8 is more hindered, which affects the charge and discharge efficiency of the battery cell and reduces the high-temperature storage performance and cycle life performance of the aqueous nickel-zinc secondary battery corresponding to Example 8. Therefore, the selection of the second type of hydrophobic material in the hydrophobic liquid and the ratio range of the mass percentage of the first type of hydrophobic material to the mass percentage of the second type of hydrophobic material should be comprehensively considered to take into account the long storage performance and cycle life performance of the aqueous nickel-zinc secondary battery, and significantly improve the cycle life performance of the aqueous nickel-zinc secondary battery.

[0094] According to the 150cyc-SOH of the aqueous nickel-zinc secondary batteries corresponding to Examples 9-13 in Tables 3 and 4, although PEEK also has a hydrophobic effect and can isolate the contact between the negative electrode plate and the electrolyte, the hydrophobic layer formed by PEEK is relatively dense, which seriously hinders the charge transfer process, making the charging and discharging of the aqueous nickel-zinc secondary battery difficult. As the content of PEEK in the hydrophobic material increases, the hydrophobic layer causes the proportion of the electrolyte in other components inside the battery to gradually increase, the internal resistance of the battery gradually increases, and the damage to the positive electrode is gradually aggravated, and the cycle life performance of the aqueous nickel-zinc secondary battery is gradually reduced.

[0095] According to the 5-day-SOC, 10-day-SOC, 15-day-SOC and 150cyc-SOH of the aqueous nickel-zinc secondary battery corresponding to the comparative examples in Table 1 and Table 2 and Examples 1-7, the high-temperature storage performance and cycle life performance of the aqueous nickel-zinc secondary battery are comprehensively considered, a hydrophobic material mixed powder prepared with PEEK and PTFE in a mass ratio of 40%:60% by mass is prepared, and a hydrophobic liquid is prepared with a mass ratio of the mixed powder to ethanol of 1:19, and the hydrophobic liquid is sprayed on the negative electrode material according to a set spraying amount to form a hydrophobic layer of mixed PEEK and PTFE. The optimal set spraying amount of the hydrophobic liquid is 8 g / m 2 -10g / m 2 .

[0096] The embodiments of the present application have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A negative electrode plate for an aqueous nickel-zinc secondary battery, characterized in that: It comprises a current collector, a negative electrode material layer disposed on at least one side of the current collector, and a hydrophobic layer covering the negative electrode material layer, wherein the hydrophobic layer is used to isolate the contact between the negative electrode material layer and the electrolyte; wherein, The hydrophobic layer includes a hydrophobic material, which includes a first type of hydrophobic material and a second type of hydrophobic material. The particle size of the first type of hydrophobic material is smaller than that of the second type of hydrophobic material. The first type of hydrophobic material includes polyetheretherketone.

2. The negative electrode sheet according to claim 1, characterized in that: The second type of hydrophobic materials includes polymethyl methacrylate and / or fluoroplastics.

3. The negative electrode sheet according to claim 2, characterized in that: The fluoroplastics include one or more of polytetrafluoroethylene, fluorinated ethylene propylene copolymer, ethylene-tetrafluoroethylene copolymer, and fluoroplastics.

4. The negative electrode sheet according to claim 1, characterized in that: The hydrophobic material and a set solvent are mixed in a set mass ratio to prepare a hydrophobic liquid, the hydrophobic liquid is sprayed on the negative electrode material layer in a set spraying amount, and the hydrophobic layer is formed on the surface of the negative electrode material layer through drying and rolling.

5. The negative electrode sheet according to claim 4, characterized in that: The mass ratio of the hydrophobic material to the set solvent is (1:19)-(1:10).

6. The negative electrode plate according to claim 5, characterized in that: The second type of hydrophobic material is polytetrafluoroethylene; wherein, In 100 grams of the hydrophobic material, the mass percentage ratio of the polyetheretherketone to the polytetrafluoroethylene is in the range of (20%:80%) to (40%:60%).

7. The negative electrode plate according to claim 6, characterized in that: The particle size of the polyetheretherketone is 2 μm-5 μm, and the particle size of the polytetrafluoroethylene is 20 μm-30 μm.

8. The negative electrode plate according to claim 6, characterized in that: The set spraying amount is 5g / m 2 -15g / m 2 ; Preferably, the set spraying amount is 5g / m 2 -10g / m 2 .

9. The negative electrode sheet according to claim 4, characterized in that: The roller pressing pressure is 1 MPa-5 MPa.

10. An aqueous nickel-zinc secondary battery, characterized in that: The invention comprises a positive electrode sheet, an electrolyte, a separator, and a negative electrode sheet as claimed in any one of claims 1 to 9.