Epitaxial structure of nitride semiconductor laser and preparation method of single crystal film
Patent Information
- Application Number
- CN202410934767.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-22
AI Technical Summary
[0004]激光器的折射率色散,高浓度载流子浓度起伏影响有源层的折射率,限制因子随波长增加而减少,导致激光器的模式增益降低;
[0043] The beneficial effects of the present invention are that: the present invention sets the lower waveguide layer as a refractive index gradient lower waveguide layer, including a first steeply changing lower waveguide layer and a second slowly changing lower waveguide layer, and controls the first steeply changing lower waveguide layer and the second gradually changing lower waveguide layer. The refractive index distribution and radiation recombination of the waveguide layer under the second gradual change Coefficient distribution, peak electron drift rate distribution, and transverse sound velocity distribution are used to improve the aging life and aging light attenuation of the laser, reduce the impurity absorption loss and carrier absorption loss of the lower wave layer, reduce the internal optical loss, and improve the surface morphology of the lower waveguide layer. Flatness and crystal quality.
Smart Images

Figure CN119009677A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor optoelectronic devices, and in particular relates to an epitaxial structure of a III-nitride semiconductor laser and a single crystal film preparation method thereof. Background Art
[0002] Lasers are widely used in laser display, laser TV, laser projector, communication, medical treatment, weapon, guidance, ranging, spectral analysis, cutting, precision welding, high-density optical storage and other fields. There are many types of lasers, and the classification methods are also diverse. There are mainly solid, gas, liquid, semiconductor and dye types of lasers; compared with other types of lasers, all-solid-state semiconductor ultraviolet lasers have the advantages of small size, high efficiency, light weight, good stability, long life, simple and compact structure, and miniaturization. There are major differences between lasers and nitride semiconductor light-emitting diodes: 1) Lasers are generated by stimulated radiation of carriers, with a small half-width of the spectrum and high brightness. The output power of a single laser can be in the W level, while nitride semiconductor light-emitting diodes are spontaneously radiated, and the output power of a single light-emitting diode is in the mW level; 2) The current density of the laser is up to KA / cm 2 , which is more than 2 orders of magnitude higher than that of nitride light-emitting diodes, resulting in stronger electron leakage, more serious Auger recombination, stronger polarization effect, more serious electron-hole mismatch, and more serious efficiency attenuation Droop effect; 3) The light-emitting diode spontaneously radiates, without external influence, and is incoherent light that transitions from high energy level to low energy level, while the laser is stimulated transition radiation, and the energy of the induced photon should be equal to the difference in energy levels of the electron transition, generating photons and induced photons with identical coherent light; 4) The principles are different: the light-emitting diode is under the action of external voltage, and the electron-hole transition to the active layer or pn junction generates radiation recombination and luminescence, while the laser needs the lasing conditions to be met before it can be lased, and the carrier inversion distribution in the active area must be met. The stimulated radiation light oscillates back and forth in the resonant cavity, and the propagation in the gain medium amplifies the light, and the threshold condition is met so that the gain is greater than the loss, and finally the laser is output.
[0003] Nitride semiconductor ultraviolet lasers have the following problems:
[0004] The refractive index dispersion of the laser, the fluctuation of high-concentration carrier concentration affects the refractive index of the active layer, and the confinement factor decreases with increasing wavelength, resulting in a decrease in the mode gain of the laser;
[0005] Increasing the thickness of the lower confinement layer can reduce the refractive index of the confinement layer, but increasing the thickness of the lower confinement layer will limit the control range of the components, which may cause cracking, bending and quality degradation.
[0006] Since the refractive index difference between GaN and AlGaN decreases with the increase of light wavelength, the thickness of the confinement layer increases when the optical confinement factor is insufficient in the blue and green light bands;
[0007] The substrate mode is characterized by a small laser spot divergence angle, a far-field image that does not satisfy the Gaussian pattern in the c-axis direction of the laser epitaxial layer, poor spot quality, and inability to focus.
[0008] The light field is dissipated, and the light field mode leaks into the substrate to form standing waves, which leads to low substrate mode suppression efficiency and poor far-field image FFP quality. Summary of the invention
[0009] The purpose of the present invention is to provide an epitaxial structure of a III-nitride semiconductor laser with a simple structure and reasonable design in order to solve the above problems.
[0010] The present invention achieves the above-mentioned purpose through the following technical solutions:
[0011] An epitaxial structure of a III-nitride semiconductor laser comprises, from bottom to top, a substrate, a lower cladding layer, a lower waveguide layer, an active layer, an upper waveguide layer, a first upper cladding layer, an electron blocking layer, and a second upper cladding layer, wherein the lower waveguide layer is a lower waveguide layer with a gradient refractive index;
[0012] The refractive index gradient lower waveguide layer includes a first steeply folded lower waveguide layer and a second gradually folded lower waveguide layer.
[0013] The refractive index distribution of the waveguide layer under the first fold steep change has a function y=(e x +e -x ) / (e x -e -x ) curve distribution; the refractive index distribution of the second gradually varying lower waveguide layer has a function y=x -a (a>1 odd number) third quadrant curve distribution;
[0014] The radiation recombination coefficient distribution of the waveguide layer under the first fold abrupt change has a function y=e x / x third quadrant curve distribution; the radiation recombination coefficient distribution of the second gradually varying lower waveguide layer has a function y=x -b (b>1 odd number) third quadrant curve distribution;
[0015] The peak electron drift velocity distribution of the waveguide layer under the first fold abrupt change has a function y=sinx / x 2 The third quadrant curve distribution; the peak electron drift rate distribution of the second gradually changing lower waveguide layer has a function y=x -c (c>1 odd number) third quadrant curve distribution;
[0016] The deformation potential distribution of the first steeply folded waveguide layer has a function y=xk / x (k>0) and a second three-quadrant curve distribution; the deformation potential distribution of the second gradually folded waveguide layer has a function y=e x / x 2 The second quadrant curve distribution;
[0017] The transverse sound velocity distribution of the first steeply folded lower waveguide layer has a second three-quadrant curve distribution of function y=xh / x (h>0); the transverse sound velocity distribution of the second gradually folded lower waveguide layer has a second three-quadrant curve distribution of function y=xd / x (d>0);
[0018] The refractive index distribution, radiation recombination coefficient distribution, peak electron drift velocity distribution, and transverse sound velocity distribution of the second gradually varying lower waveguide layer have the following relationship: d≤b≤a≤c.
[0019] Further, the descending angle of the peak position of the refractive index of the first steeply folded lower waveguide layer toward the lower cladding layer is α, the descending angle of the peak position of the refractive index of the second gradually folded lower waveguide layer toward the lower cladding layer is β, and the rising angle of the valley position of the refractive index of the second gradually folded lower waveguide layer toward the active layer is γ, wherein 20°≤β≤45°≤γ≤60°≤α≤90°, and the angle is the tangent inclination angle of the curve;
[0020] The peak position of the radiation recombination coefficient of the first steeply folded lower waveguide layer has a descending angle of θ toward the lower cladding layer, the peak position of the radiation recombination coefficient of the second gradually folded lower waveguide layer has a descending angle of δ toward the lower cladding layer, and the valley position of the radiation recombination coefficient of the second gradually folded lower waveguide layer has a rising angle of σ toward the active layer, wherein 10°≤δ≤45°≤σ≤60°≤θ≤90°, and the angle is the tangent inclination angle of the curve;
[0021] The rising angle of the valley position of the deformation potential of the first steeply folded lower waveguide layer toward the lower cladding layer is φ, the rising angle of the valley position of the deformation potential of the second gradually folded lower waveguide layer toward the lower cladding layer is ψ, and the falling angle of the peak position of the deformation potential of the second gradually folded lower waveguide layer toward the active layer is μ, wherein 15°≤ψ≤45°≤μ≤60°≤φ≤90°, and the angle is the tangent inclination angle of the curve;
[0022] The rising angle of the valley position of the transverse sound velocity of the first steeply folded lower waveguide layer toward the lower cladding layer is υ, the rising angle of the valley position of the transverse sound velocity of the second gradually folded lower waveguide layer toward the lower cladding layer is ρ, and the descending angle of the peak position of the transverse sound velocity of the second gradually folded lower waveguide layer toward the active layer is ω, wherein: 5°≤ρ≤45°≤ω≤60°≤υ≤90°, and the angle is the tangent inclination angle of the curve;
[0023] The descending angle of the peak position of the peak electron drift rate of the first steeply-change lower waveguide layer toward the lower cladding layer is ε, the descending angle of the peak position of the peak electron drift rate of the second gradually-change lower waveguide layer toward the lower cladding layer is η, and the rising angle of the valley position of the peak electron drift rate of the second gradually-change lower waveguide layer toward the active layer is κ, wherein 25°≤η≤45°≤κ≤60°≤ε≤90°, and the angle is the tangent inclination angle of the curve.
[0024] The refractive index, radiation recombination coefficient, and descending angle of the peak position of the peak electron drift velocity of the waveguide layer under the first fold steep change toward the lower cladding layer, and the rising angle of the deformation potential and the valley position of the transverse sound velocity of the waveguide layer under the first fold steep change toward the lower cladding layer have the following relationship: 25°≤υ≤θ≤φ≤α≤ε≤90°, where the angle is the tangent inclination angle of the curve;
[0025] The refractive index, radiation recombination coefficient, and descending angle of the peak position of the peak electron drift velocity of the second gradually varying lower waveguide layer toward the lower cladding layer, and the rising angle of the deformation potential and the valley position of the transverse sound velocity of the second gradually varying lower waveguide layer toward the lower cladding layer have the following relationship: 5°≤ρ≤ψ≤δ≤β≤η≤90°, where the angle is the tangent inclination angle of the curve;
[0026] The refractive index, radiation recombination coefficient, and rising angle of the valley position of the peak electron drift velocity of the second gradually varying lower waveguide layer toward the active layer, and the deformation potential and the descending angle of the peak position of the transverse sound velocity of the second gradually varying lower waveguide layer toward the active layer have the following relationship: 15°≤ω≤σ≤μ≤γ≤κ≤90°, where the angle is the tangent inclination angle of the curve.
[0027] Further, the angle of descent of the refractive index, radiation recombination coefficient, and peak position of the peak electron drift velocity of the first steeply folded lower waveguide layer toward the lower cladding layer, the angle of descent of the deformation potential and the valley position of the transverse sound velocity of the first steeply folded lower waveguide layer toward the lower cladding layer, the angle of descent of the refractive index, radiation recombination coefficient, and peak position of the peak electron drift velocity of the second gradually folded lower waveguide layer toward the lower cladding layer, the angle of descent of the deformation potential and the valley position of the transverse sound velocity of the second gradually folded lower waveguide layer toward the lower cladding layer, the angle of descent of the refractive index, radiation recombination coefficient, and valley position of the peak electron drift velocity of the second gradually folded lower waveguide layer toward the active layer, and the angle of descent of the deformation potential and the peak position of the transverse sound velocity of the second gradually folded lower waveguide layer toward the active layer have the following relationship: 5°≤ρ≤ψ≤δ≤β≤η≤ω≤σ≤μ≤γ≤κ≤υ≤θ≤φ≤α≤ε≤90°, where the angle is the tangent inclination angle of the curve.
[0028] The first steeply folded lower waveguide layer and the second gradually folded lower waveguide layer are any one or any combination of InGaN, GaN, InN, AlInGaN, AlInN, InGaN / GaN superlattice, InGaN / AlInGaN superlattice, InGaN / AlInN superlattice, GaN / AlInGaN superlattice, and GaN / AlInGaN superlattice, and have a thickness of 5 to 1000 nm.
[0029] The active layer is any one or any combination of GaN, InGaN, InN, AlInN, AlGaN, AlInGaN, AlN, GaAs, GaP, InP, AlGaAs, AlInGaAs, AlGaInP, InGaAs, InGaAsN, AlInAs, AlInP, AlGaP, InGaP, GaSb, InSb, InAs, InAsSb, AlGaSb, AlSb, InGaSb, AlGaAsSb, InGaAsSb, SiC, Ga2O3, BN, and diamond, and has a thickness of 10 to 100 angstroms. The barrier layer of the active layer is GaN, InGaN, InN, AlInN, AlGaN, AlInGaN, AlN, GaAs, GaP, InP, AlGaAs, AlInGaAs, AlGaInP, InGaAs, InGaAsN, AlIn Any one or any combination of nAs, Al InP, Al GaP, InGaP, GaSb, InSb, InAs, InAsSb, Al GaSb, Al Sb, InGaSb, Al GaAsSb, InGaAsSb, SiC, Ga2O3, BN, diamond, with a thickness of 10 to 200 angstroms;
[0030] The lower cladding layer, the lower waveguide layer, the first upper cladding layer, the electron blocking layer, and the second upper cladding layer are any one or any combination of GaN, InGaN, InN, Al InN, Al GaN, Al InGaN, Al N, GaAs, GaP, InP, Al GaAs, Al InGaAs, AlGaInP, InGaAs, InGaAsN, Al InAs, Al InP, Al GaP, InGaP, GaSb, InSb, InAs, InAsSb, Al GaSb, Al Sb, InGaSb, Al GaAsSb, InGaAsSb, SiC, Ga2O3, BN, and diamond.
[0031] The substrate includes any one of sapphire, silicon, Ge, SiC, Al N, GaN, GaAs, InP, InAs, GaSb, sapphire / SiO2 composite substrate, Mo, TiW, CuW, Cu, sapphire / Al N composite substrate, diamond, graphene, sapphire / SiNx, sapphire / SiO2 / SiNx composite substrate, sapphire / SiNx / SiO2 composite substrate, magnesium aluminum spinel MgAl2O4, MgO, ZnO, ZrB2, LiAlO2 and LiGaO2 composite substrate.
[0032] A method for preparing a III-nitride semiconductor laser single crystal thin film comprises the following steps:
[0033] S1: introducing the substrate into the MOCVD metal organic chemical vapor deposition reaction chamber;
[0034] S2: Set the temperature and pressure of the reaction chamber;
[0035] S3: Introducing the required reaction gases one by one through the gas flow controller, including TMGa, TEGa, TMAl, TMI n, NH3, N2 and H2;
[0036] S4: setting the rotation speed of the substrate;
[0037] S5: Introducing the required doping elements one by one through a gas flow controller, including any one of Cp2Mg, SiH4 or disilane;
[0038] S6: growing a lower cladding layer, a lower waveguide layer, an active layer, an upper waveguide layer, a first upper cladding layer, an electron blocking layer, and a second upper cladding layer in sequence;
[0039] The lower waveguide layer is a lower waveguide layer with a gradient refractive index; the lower waveguide layer with a gradient refractive index includes a first steeply folded lower waveguide layer and a second gradually folded lower waveguide layer.
[0040] Further, in step S2, the temperature of the reaction chamber is set to 500-1200° C., and the growth pressure in the reaction chamber is controlled to be in the range of 100-550 Torr;
[0041] In step S3, the V / III ratio is controlled to be 100 to 80000;
[0042] In step S4, the substrate is rotated at a speed of 500 to 1300 revolutions.
[0043] The beneficial effects of the present invention are as follows: the present invention improves the aging life and aging optical attenuation of the laser, reduces the impurity absorption loss and carrier absorption loss of the lower wave layer, reduces the internal optical loss, and improves the surface morphology flatness and crystal quality of the lower waveguide layer by setting the lower waveguide layer as a refractive index gradient lower waveguide layer, including a first steeply folded lower waveguide layer and a second gradually folded lower waveguide layer, and controlling the refractive index distribution, radiation recombination coefficient distribution, peak electron drift rate distribution, and lateral sound velocity distribution of the first steeply folded lower waveguide layer and the second gradually folded lower waveguide layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 This is a SIMS secondary ion mass spectrum diagram of the structure of a semiconductor laser element according to an embodiment of the present invention (partially enlarged diagram);
[0045] Figure 2 It is a SIMS secondary ion mass spectrum of the structure of a semiconductor laser element according to an embodiment of the present invention;
[0046] Figure 3 is a schematic structural diagram of a semiconductor laser element according to an embodiment of the present invention;
[0047] Figure 4 This is a TEM lens electron microscope image of a semiconductor laser element according to an embodiment of the present invention;
[0048] Figure 5 This is a TEM lens electron microscope image (partial magnified image) of a semiconductor laser element according to an embodiment of the present invention;
[0049] Figure 6 This is a TEM lens electron microscope image (partial magnified image) of a semiconductor laser element according to an embodiment of the present invention.
[0050] In the figure: 100, substrate; 101, lower cladding layer; 102, lower waveguide layer; 102a, first steeply folded lower waveguide layer; 102b, second gradually folded lower waveguide layer; 103, active layer; 104, upper waveguide layer; 105, first upper cladding layer; 106, electron blocking layer; 107, second upper cladding layer. DETAILED DESCRIPTION
[0051] The present application is further described in detail below in conjunction with the accompanying drawings. It is necessary to point out here that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technical personnel in this field can make some non-essential improvements and adjustments to the present application based on the above application content.
[0052] like Figure 1-Figure 6As shown, an epitaxial structure of a III-nitride semiconductor laser includes, from bottom to top, a substrate 100, a lower cladding layer 101, a lower waveguide layer 102, an active layer 103, an upper waveguide layer 104, a first upper cladding layer 105, an electron blocking layer 106, and a second upper cladding layer 107, wherein the lower waveguide layer 102 is a lower waveguide layer with a gradient refractive index;
[0053] The refractive index gradient lower waveguide layer includes a first steeply folded lower waveguide layer 102a and a second gradually folded lower waveguide layer 102b.
[0054] The refractive index distribution of the first fold steep lower waveguide layer 102a has a function y=(e x +e -x ) / (e x -e -x ) curve distribution; the refractive index distribution of the second gradually varying lower waveguide layer 102b has a function y=x -a (a>1 odd number) third quadrant curve distribution;
[0055] The distribution of refractive index can affect the propagation behavior of light. The refractive index distribution in the form of a hyperbolic tangent function usually means that there is a gradient refractive index in the waveguide structure. This gradient refractive index distribution can be used to achieve some special optical functions.
[0056] The radiation recombination coefficient distribution of the first fold steep change waveguide layer 102a has a function y=e x / x third quadrant curve distribution; the radiation recombination coefficient distribution of the second gradually varying lower waveguide layer 102b has a function y=x -b (b>1 odd number) third quadrant curve distribution;
[0057] The radiative recombination coefficient is a physical quantity that describes the rate at which electrons and holes in semiconductor materials recombine through radiation. In semiconductor devices, radiative recombination is an important way for electrons and holes to recombine, and the energy generated is released in the form of photons.
[0058] The peak electron drift velocity distribution of the first fold lower waveguide layer 102a has a function y=sinx / x 2 The third quadrant curve distribution; the peak electron drift rate distribution of the second gradually changing lower waveguide layer 102b has a function y=x -c (c>1 odd number) third quadrant curve distribution;
[0059] The deformation potential distribution of the first steeply folded lower waveguide layer 102a has a function y=xk / x (k>0) of the second three-quadrant curve distribution; the deformation potential distribution of the second gradually folded lower waveguide layer 102b has a function y=e x / x 2 The second quadrant curve distribution;
[0060] The transverse sound velocity distribution of the first steeply folded lower waveguide layer 102a has a second three-quadrant curve distribution of function y=xh / x (h>0); the transverse sound velocity distribution of the second gradually folded lower waveguide layer 102b has a second three-quadrant curve distribution of function y=xd / x (d>0);
[0061] The refractive index distribution, radiation recombination coefficient distribution, peak electron drift velocity distribution, and transverse sound velocity distribution of the second gradually varying lower waveguide layer 102b have the following relationship: d≤b≤a≤c.
[0062] Further, the descending angle of the peak position of the refractive index of the first steeply folded lower waveguide layer 102a toward the lower cladding layer 101 is α, the descending angle of the peak position of the refractive index of the second gradually folded lower waveguide layer 102b toward the lower cladding layer 101 is β, and the rising angle of the valley position of the refractive index of the second gradually folded lower waveguide layer 102b toward the active layer 103 is γ, wherein 20°≤β≤45°≤γ≤60°≤α≤90°, and the angle is the tangent inclination angle of the curve;
[0063] Design the refractive index gradient trend and change angle of the lower waveguide layer, regulate the light field distribution of the lower waveguide layer, suppress refractive index dispersion and light field dissipation, alleviate the problem that the refractive index difference decreases with the increase of light wavelength, improve the optical confinement factor, improve the restrictiveness and concentration of the longitudinal light field, suppress substrate mode leakage, increase the vertical divergence angle of the main light spot, make the far-field light spot elliptical, improve the laser beam quality factor, and enhance the optical confinement and mode gain of the lower waveguide layer.
[0064] The peak position of the radiation recombination coefficient of the first steeply folded lower waveguide layer 102a decreases at an angle of θ toward the lower cladding layer 101, the peak position of the radiation recombination coefficient of the second gradually folded lower waveguide layer 102b decreases at an angle of δ toward the lower cladding layer 101, and the valley position of the radiation recombination coefficient of the second gradually folded lower waveguide layer 102b increases at an angle of σ toward the active layer 103, wherein 10°≤δ≤45°≤σ≤60°≤θ≤90°, and the angle is the tangent inclination angle of the curve;
[0065] Design the radiation recombination rate trend and change angle of the lower waveguide layer, reduce the non-radiative recombination centers of various impurities and defects, reduce internal optical absorption losses, and inhibit the migration and proliferation of impurities and defects during the aging process, thereby improving the aging life and aging optical attenuation of the laser.
[0066] The rising angle of the valley position of the deformation potential of the first steeply folded lower waveguide layer 102a toward the lower cladding layer 101 is φ, the rising angle of the valley position of the deformation potential of the second gradually folded lower waveguide layer 102b toward the lower cladding layer 101 is ψ, and the falling angle of the peak position of the deformation potential of the second gradually folded lower waveguide layer 102b toward the active layer 103 is μ, wherein: 15°≤ψ≤45°≤μ≤60°≤φ≤90°, the angle is the tangent inclination angle of the curve;
[0067] The deformation potential trend and change angle of the lower waveguide layer 102 are designed to reduce the lattice mismatch and stress between the lower waveguide layer 102 and the lower cladding layer 101 and the active layer 103, reduce the structural defects such as I n segregation, dislocation, stacking fault and pores of the lower waveguide layer 102, improve the surface morphology flatness and crystal quality of the lower waveguide layer, and then improve the surface flatness and interface state of the active layer, improve the aging life and aging light attenuation of the laser, and reduce the abnormal proportion of cracking, bending and edge and angle collapse of the laser.
[0068] The rising angle of the valley position of the transverse sound velocity of the first steeply folded lower waveguide layer 102a toward the lower cladding layer 101 is υ, the rising angle of the valley position of the transverse sound velocity of the second gradually folded lower waveguide layer 102b toward the lower cladding layer 101 is ρ, and the descending angle of the peak position of the transverse sound velocity of the second gradually folded lower waveguide layer 102b toward the active layer 103 is ω, wherein: 5°≤ρ≤45°≤ω≤60°≤υ≤90°, the angle is the tangent inclination angle of the curve;
[0069] The lateral sound velocity trend and change angle of the lower waveguide layer 102 are designed to regulate the phonon distribution and phonon transport of the laser, suppress light field dissipation and substrate mode leakage, improve the far-field FFP image quality, make the far-field image close to the Gaussian pattern, and improve the laser beam quality factor.
[0070] The descending angle of the peak position of the peak electron drift rate of the first steeply folded lower waveguide layer 102a toward the lower cladding layer 101 is ε, the descending angle of the peak position of the peak electron drift rate of the second gradually folded lower waveguide layer 102b toward the lower cladding layer 101 is η, and the rising angle of the valley position of the peak electron drift rate of the second gradually folded lower waveguide layer 102b toward the active layer 103 is κ, wherein 25°≤η≤45°≤κ≤60°≤ε≤90°, and the angle is the tangent inclination angle of the curve;
[0071] The peak electron drift rate trend and change angle of the lower waveguide layer 102 are designed to regulate the electron and hole transport of the lower waveguide layer, reduce the impurity absorption loss and carrier absorption loss of the lower waveguide layer, and reduce the internal optical loss.
[0072] The refractive index, radiation recombination coefficient, and descending angle of the peak position of the peak electron drift velocity of the waveguide layer 102a under the first fold steep change toward the lower cladding layer 101, and the rising angle of the deformation potential and the valley position of the transverse sound velocity of the waveguide layer 102a under the first fold steep change toward the lower cladding layer 101 have the following relationship: 25°≤υ≤θ≤φ≤α≤ε≤90°, where the angle is the tangent inclination angle of the curve;
[0073] The refractive index, radiation recombination coefficient, and descending angle of the peak position of the peak electron drift velocity of the second gradually varying lower waveguide layer 102b toward the lower cladding layer 101, and the rising angle of the deformation potential and the valley position of the transverse sound velocity of the second gradually varying lower waveguide layer 102b toward the lower cladding layer 101 have the following relationship: 5°≤ρ≤ψ≤δ≤β≤η≤90°, where the angle is the tangent inclination angle of the curve;
[0074] The refractive index, radiation recombination coefficient, and rising angle of the valley position of the peak electron drift velocity of the second gradually varying lower waveguide layer 102b toward the active layer 103, and the decreasing angle of the deformation potential and the peak position of the transverse sound velocity of the second gradually varying lower waveguide layer 102b toward the active layer 103 have the following relationship: 15°≤ω≤σ≤μ≤γ≤κ≤90°, where the angle is the tangent inclination angle of the curve.
[0075] By designing the change angle and distribution of the refractive index and radiation recombination rate, the light field distribution of the lower waveguide layer is regulated, the refractive index dispersion and light field dissipation are suppressed, the trend of the laser limitation factor decreasing with wavelength is reduced, and the laser mode gain is improved; at the same time, the change angle and distribution of the peak electron drift rate, deformation potential, and transverse sound velocity are designed to regulate the electron and phonon transport of the lower waveguide layer, reduce the impurity absorption loss and carrier absorption loss of the lower wave layer, reduce the influence of carrier concentration fluctuations on the refractive index of the active layer, improve the restrictiveness and concentration of the longitudinal light field, suppress substrate mode leakage, increase the vertical divergence angle of the main light spot, make the far-field light spot elliptical, and improve the laser beam quality factor.
[0076] Furthermore, the refractive index, radiation recombination coefficient, and peak position of the peak electron drift velocity of the first steeply folded lower waveguide layer 102a are decreased at an angle toward the lower cladding layer 101, the deformation potential of the first steeply folded lower waveguide layer 102a, and the valley position of the transverse sound velocity are increased at an angle toward the lower cladding layer 101, the refractive index, radiation recombination coefficient, and peak position of the peak electron drift velocity of the second gradually folded lower waveguide layer 102b are decreased at an angle toward the lower cladding layer 101, and the deformation potential of the second gradually folded lower waveguide layer 102b is increased at an angle toward the lower cladding layer 101. , the rising angle of the valley position of the transverse sound velocity toward the lower cladding layer 101, the rising angle of the valley position of the refractive index, the radiation recombination coefficient, and the peak electron drift velocity of the second gradually varying lower waveguide layer 102b toward the active layer 103, and the deformation potential of the second gradually varying lower waveguide layer 102b and the descending angle of the peak position of the transverse sound velocity toward the active layer 103 have the following relationship: 5°≤ρ≤ψ≤δ≤β≤η≤ω≤σ≤μ≤γ≤κ≤υ≤θ≤φ≤α≤ε≤90°, where the angle is the tangent inclination angle of the curve.
[0077] The first steeply folded lower waveguide layer 102a and the second gradually folded lower waveguide layer 102b are any one or any combination of InGaN, GaN, InN, AlInGaN, AlInN, InGaN / GaN superlattice, InGaN / AlInGaN superlattice, InGaN / AlInGaN superlattice, GaN / AlInGaN superlattice, and GaN / AlInGaN superlattice, and have a thickness of 5 to 1000 nm.
[0078] The active layer 103 is any one or any combination of GaN, InGaN, InN, AlInN, AlGaN, AlInGaN, AlN, GaAs, GaP, InP, AlGaAs, AlInGaAs, AlGaInP, InGaAs, InGaAsN, AlInAs, AlInP, AlGaP, InGaP, GaSb, InSb, InAs, InAsSb, AlGaSb, AlSb, InGaSb, AlGaAsSb, InGaAsSb, InGaAsSb, SiC, Ga2O3, BN, and diamond, and has a thickness of 10 to 100 angstroms. The barrier layer of the active layer 103 is GaN, InGaN, InN, AlInN, AlGaN, AlInGaN, AlN, GaAs, GaP, InP, AlGaAs, AlInGaAs, AlGaInP, InGaAs, I Any one or any combination of nGaAsN, Al InAs, Al InP, Al GaP, InGaP, GaSb, InSb, InAs, InAsSb, Al GaSb, Al Sb, InGaSb, Al GaAsSb, InGaAsSb, SiC, Ga2O3, BN, and diamond, with a thickness of 10 to 200 angstroms;
[0079] The lower cladding layer 101, the lower waveguide layer 102, the first upper cladding layer 105, the electron blocking layer 106, and the second upper cladding layer 107 are any one or any combination of GaN, InGaN, InN, AlInN, AlGaN, AlInGaN, AlN, GaAs, GaP, InP, AlGaAs, AlInGaAs, AlGaInP, InGaAs, InGaAsN, AlInAs, AlInP, AlGaP, InGaP, GaSb, InSb, InAs, InAsSb, AlGaSb, AlSb, InGaSb, AlGaAsSb, InGaAsSb, SiC, Ga2O3, BN, and diamond.
[0080] The substrate 100 includes any one of sapphire, silicon, Ge, SiC, Al N, GaN, GaAs, InP, InAs, GaSb, sapphire / SiO2 composite substrate, Mo, TiW, CuW, Cu, sapphire / Al N composite substrate, diamond, graphene, sapphire / SiNx, sapphire / SiO2 / SiNx composite substrate, sapphire / SiNx / SiO2 composite substrate, magnesium aluminum spinel MgAl2O4, MgO, ZnO, ZrB2, LiAlO2 and LiGaO2 composite substrates.
[0081] In order to highlight the technical advantages of the present technical solution, this embodiment compares the performance of the laser element proposed by the present invention with that of a traditional laser element. The comparison results can be seen in Table 1.
[0082] The structure of the conventional laser is substrate, lower cladding layer, lower waveguide layer, active layer, upper waveguide layer, first upper cladding layer, electron blocking layer, second upper cladding layer; the structure of the laser of the present invention is substrate, lower cladding layer, first steeply folded lower waveguide layer, second gradually folded lower waveguide layer, active layer, upper waveguide layer, first upper cladding layer, electron blocking layer, second upper cladding layer;
[0083] The laser element of the present invention is tested by using a laser chip test device, wherein the laser element is designed with a ridge width of 45um, a cavity length of 1200um, a test current of 0-4A ampere pulse or continuous mode test, and a test environment temperature of 25°C. Then, the laser light power signal is collected by an integrating sphere, and the laser signal is tested at a variable angle, thereby testing the beam quality factor, vertical divergence angle, and limiting factor.
[0084] When conducting the aging life test, the sample is placed in an oven for aging test, where the aging temperature is 65°C and the aging current is 3A. Then the aging light attenuation at different aging times is tested, and the cracking, edge collapse and angle collapse failure ratios during the aging process are counted.
[0085] Table 1
[0086] project Conventional laser Laser of the present invention Range of change <![CDATA[Beam quality factor M 2 > 1.89 1.21 56% 1000H aging light decay 13.2% 7.1% 46% Abnormal proportion of cracking, edge and corner collapse 43PPM 14PPM 67% Limiting Factor 1.50% 2.46% 64% Vertical divergence 10~40° 30~70°
[0087] By comparison, it can be found that the beam quality factor of the III-nitride semiconductor laser proposed in the present invention is 1.89M·m·s compared with the traditional laser. 2 Reduced to 1.21M 2 , the change is 56%. The beam quality factor is usually used to describe the spatial structure and focusing performance of the laser beam. The closer the value is to 1, the higher the quality of the laser beam is, that is, the beam is closer to the ideal Gaussian beam. Therefore, from 1.89M 2 Reduced to 1.21M2 It means that the quality of the light beam is improved, providing greater flexibility and possibilities for the design of optical devices; the 1000H aging light attenuation is reduced from 13.2% to 7.1%, with a change range of 46%. The reduction in the light attenuation rate means that the performance of optical devices or systems degrades more slowly, thus extending the service life of the product; the abnormal proportion of cracking, edge collapse and angle collapse is reduced from 43PPM to 14PPM, with a change range of 67%. The reduction in the abnormal proportion means reducing production losses, improving production efficiency and production line operation efficiency, thereby reducing production costs; the limiting factor is increased from 1.50% to 2.46%, with a change range of 64%, which improves the performance and reliability of the device, and can reduce the dispersion of device parameters, making the performance differences between devices smaller, and the vertical divergence angle is increased from 10~40° to 30~70°.
[0088] A method for preparing a III-nitride semiconductor laser single crystal thin film comprises the following steps:
[0089] S1: introducing the substrate 100 into the MOCVD metal organic chemical vapor deposition reaction chamber;
[0090] S2: Set the temperature and pressure of the reaction chamber;
[0091] S3: Introducing the required reaction gases one by one through the gas flow controller, including TMGa, TEGa, TMAl, TMI n, NH3, N2 and H2;
[0092] S4: setting the rotation speed of the substrate 100;
[0093] S5: Introducing the required doping elements one by one through a gas flow controller, including any one of Cp2Mg, SiH4 or disilane;
[0094] S6: growing the lower cladding layer 101, the lower waveguide layer 102, the active layer 103, the upper waveguide layer 104, the first upper cladding layer 105, the electron blocking layer 106 and the second upper cladding layer 107 in sequence;
[0095] The lower waveguide layer 102 is a lower waveguide layer 102 with a gradient refractive index; the lower waveguide layer 102 with a gradient refractive index includes a first steeply folded lower waveguide layer 102a and a second gradually folded lower waveguide layer 102b.
[0096] Further, in step S2, the temperature of the reaction chamber is set to 500-1200° C., and the growth pressure in the reaction chamber is controlled to be in the range of 100-550 Torr;
[0097] In step S3, the V / III ratio is controlled to be 100 to 80000;
[0098] In step S4, the substrate 100 is rotated at a speed of 500 to 1300 revolutions.
[0099] In a specific embodiment, the Al / Ga atomic ratio is controlled to change the injection curve to y=g x (g>1) curve distribution, so that the refractive index distribution of the waveguide layer 102a under the first fold steep change has a function y=(e x +e -x ) / (e x -e -x ) curve distribution;
[0100] By controlling the ratio of In / Ga atoms, the injection curve changes to y=x -a (a>1 odd number) curve distribution, so that the refractive index distribution of the second graded lower waveguide layer 102b has a function y=x -a (a>1 odd number) third quadrant curve distribution;
[0101] The refractive index gradient trend and change angle of the lower waveguide layer 102 are designed, the light field distribution of the lower waveguide layer 102 is regulated, the refractive index dispersion and light field dissipation are suppressed, the problem that the refractive index difference decreases with the increase of light wavelength is alleviated, the optical confinement factor is improved, the confinement and concentration of the longitudinal light field are improved, the substrate 100 mode leakage is suppressed, the vertical divergence angle of the main light spot light field is improved, the far-field light spot is made elliptical, the laser beam quality factor is improved, and the optical confinement and mode gain of the lower waveguide layer 102 are enhanced.
[0102] By controlling the Al / Ga atomic ratio, the injection curve changes to y=xe x The curve distribution makes the radiation recombination coefficient distribution of the waveguide layer 102a under the first fold steep change have a function y=e x / xThe third quadrant curve distribution;
[0103] By controlling the ratio of In / Ga atoms, the injection curve changes to y=x -b (b>1 odd number) curve distribution, so that the radiation recombination coefficient distribution of the second graded lower waveguide layer 102b has a function y=x -b (b>1 odd number) third quadrant curve distribution;
[0104] The radiation recombination rate trend and change angle of the lower waveguide layer 102 are designed to reduce the non-radiative recombination centers of various impurities and defects, reduce internal optical absorption losses, and inhibit the migration and proliferation of impurities and defects during the aging process, thereby improving the aging life and aging optical attenuation of the laser.
[0105] By controlling the Al / Ga atomic ratio, the implantation curve is a function of y=sinx / x 2The curve distribution makes the peak electron drift velocity distribution of the waveguide layer 102a under the first fold steep change have the function y=sinx / x 2 The third quadrant curve distribution;
[0106] By controlling the ratio of In / Ga atoms, the injection curve changes to y=x -c (c>1 odd number) curve distribution, so that the peak electron drift velocity distribution of the second graded lower waveguide layer 102b has a function y=x -c (c>1 odd number) third quadrant curve distribution;
[0107] The peak electron drift rate trend and change angle of the lower waveguide layer 102 are designed to regulate the electron and hole transport of the lower waveguide layer 102, reduce the lower waveguide layer impurity absorption loss and carrier absorption loss, and reduce internal optical loss.
[0108] By controlling the Al / Ga atomic ratio injection variation curve to be a function y=xm / x (m>0) curve distribution, the deformation potential distribution of the first fold lower waveguide layer 102a has a second three-quadrant curve distribution of a function y=xk / x (h>0);
[0109] By controlling the ratio of In / Ga atoms, the injection curve changes to y=e x / x curve distribution, so that the deformation potential distribution of the second gradually varying lower waveguide layer 102b has a function y=e x / x 2 The second quadrant curve distribution;
[0110] The deformation potential trend and change angle of the lower waveguide layer 102 are designed to reduce the lattice mismatch and stress between the lower waveguide layer 102 and the lower cladding layer 101 and the active layer 103, reduce the structural defects such as I n segregation, dislocation, stacking fault and pores of the lower waveguide layer 102, improve the surface morphology flatness and crystal quality of the lower waveguide layer 102, and then improve the surface flatness and interface state of the active layer 103, improve the aging life and aging light attenuation of the laser, and reduce the abnormal proportion of cracking, bending and edge and angle collapse of the laser.
[0111] By controlling the Al / Ga atomic ratio injection variation curve to be a function y=xj / x (j>0) curve distribution, the lateral sound velocity distribution of the first fold lower waveguide layer 102a has a function y=xh / x (h>0) second three-quadrant curve distribution;
[0112] By controlling the In / Ga atomic ratio injection variation curve to be a function y=arccotx curve distribution, the lateral acoustic velocity distribution of the second gradually varying lower waveguide layer 102b has a second three-quadrant curve distribution of a function y=xd / x (d>0);
[0113] The lateral sound velocity trend and change angle of the lower waveguide layer 102 are designed to regulate the phonon distribution and phonon transport of the laser, suppress the light field dissipation and substrate 100 mode leakage, improve the far-field FFP image quality, make the far-field image close to the Gaussian pattern, and improve the laser beam quality factor.
[0114] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. An epitaxial structure of a III-nitride semiconductor laser, comprising, from bottom to top, a substrate, a lower cladding layer, a lower waveguide layer, an active layer, an upper waveguide layer, a first upper cladding layer, an electron blocking layer, and a second upper cladding layer, It is characterized in that The lower waveguide layer is composed of a first steeply folded lower waveguide layer and a second gradually folded lower waveguide layer; The descending angle of the peak position of the refractive index of the first steeply folded lower waveguide layer toward the lower cladding layer is α, the descending angle of the peak position of the refractive index of the second gradually folded lower waveguide layer toward the lower cladding layer is β, and the rising angle of the valley position of the refractive index of the second gradually folded lower waveguide layer toward the active layer is γ, wherein 20°≤β≤45°≤γ≤60°≤α≤90°, and the angle is the tangent inclination angle of the curve; The descending angle of the peak position of the radiation recombination coefficient of the first steeply-change lower waveguide layer toward the lower cladding layer is θ, the descending angle of the peak position of the radiation recombination coefficient of the second gradually-change lower waveguide layer toward the lower cladding layer is δ, and the rising angle of the valley position of the radiation recombination coefficient of the second gradually-change lower waveguide layer toward the active layer is σ, wherein 10°≤δ≤45°≤σ≤60°≤θ≤90°, and the angle is the tangent inclination angle of the curve.
2. The epitaxial structure of a III-nitride semiconductor laser according to claim 1, It is characterized in that The rising angle of the valley position of the deformation potential of the first steeply folded lower waveguide layer toward the lower cladding layer is φ, the rising angle of the valley position of the deformation potential of the second gradually folded lower waveguide layer toward the lower cladding layer is ψ, and the descending angle of the peak position of the deformation potential of the second gradually folded lower waveguide layer toward the active layer is μ, wherein 15°≤ψ≤45°≤μ≤60°≤φ≤90°, and the angle is the tangent inclination angle of the curve.
3. The epitaxial structure of a III-nitride semiconductor laser according to claim 2, It is characterized in that The rising angle of the valley position of the transverse sound velocity of the first steeply-change lower waveguide layer toward the lower cladding layer is υ, the rising angle of the valley position of the transverse sound velocity of the second gradually-change lower waveguide layer toward the lower cladding layer is ρ, and the descending angle of the peak position of the transverse sound velocity of the second gradually-change lower waveguide layer toward the active layer is ω, wherein 5°≤ρ≤45°≤ω≤60°≤υ≤90°, and the angle is the tangent inclination angle of the curve.
4. The epitaxial structure of a III-nitride semiconductor laser according to claim 3, It is characterized in that The descending angle of the peak position of the peak electron drift rate of the first steeply-change lower waveguide layer toward the lower cladding layer is ε, the descending angle of the peak position of the peak electron drift rate of the second gradually-change lower waveguide layer toward the lower cladding layer is η, and the rising angle of the valley position of the peak electron drift rate of the second gradually-change lower waveguide layer toward the active layer is κ, wherein 25°≤η≤45°≤κ≤60°≤ε≤90°, and the angle is the tangent inclination angle of the curve.
5. The epitaxial structure of a III-nitride semiconductor laser according to claim 4, It is characterized in that The refractive index, radiation recombination coefficient, and descending angle of the peak position of the peak electron drift velocity of the waveguide layer under the first fold steep change toward the lower cladding layer, and the rising angle of the deformation potential and the valley position of the transverse sound velocity of the waveguide layer under the first fold steep change toward the lower cladding layer have the following relationship: 25°≤υ≤θ≤φ≤α≤ε≤90°, where the angle is the tangent inclination angle of the curve; The refractive index, radiation recombination coefficient, and descending angle of the peak position of the peak electron drift velocity of the second gradually varying lower waveguide layer toward the lower cladding layer, and the rising angle of the deformation potential and the valley position of the transverse sound velocity of the second gradually varying lower waveguide layer toward the lower cladding layer have the following relationship: 5°≤ρ≤ψ≤δ≤β≤η≤90°, where the angle is the tangent inclination angle of the curve; The refractive index, radiation recombination coefficient, and rising angle of the valley position of the peak electron drift velocity of the second gradually varying lower waveguide layer toward the active layer, and the deformation potential and the descending angle of the peak position of the transverse sound velocity of the second gradually varying lower waveguide layer toward the active layer have the following relationship: 15°≤ω≤σ≤μ≤γ≤κ≤90°, where the angle is the tangent inclination angle of the curve.
6. The epitaxial structure of a III-nitride semiconductor laser according to claim 5, It is characterized in that The descending angle of the refractive index, radiation recombination coefficient, and peak position of the peak electron drift velocity of the first steeply folded lower waveguide layer toward the lower cladding layer, the rising angle of the deformation potential and the valley position of the transverse sound velocity of the first steeply folded lower waveguide layer toward the lower cladding layer, the descending angle of the refractive index, radiation recombination coefficient, and peak position of the peak electron drift velocity of the second gradually folded lower waveguide layer toward the lower cladding layer, the rising angle of the deformation potential and the valley position of the transverse sound velocity of the second gradually folded lower waveguide layer toward the lower cladding layer, the rising angle of the refractive index, radiation recombination coefficient, and valley position of the peak electron drift velocity of the second gradually folded lower waveguide layer toward the active layer, and the descending angle of the deformation potential and the peak position of the transverse sound velocity of the second gradually folded lower waveguide layer toward the active layer have the following relationship: 5°≤ρ≤ψ≤δ≤β≤η≤ω≤σ≤μ≤γ≤κ≤υ≤θ≤φ≤α≤ε≤90°, and the angle is the tangent inclination angle of the curve.
7. The epitaxial structure of a III-nitride semiconductor laser according to claim 6, It is characterized in that The first steeply folded lower waveguide layer and the second gradually folded lower waveguide layer are any one or any combination of InGaN, GaN, InN, AlInGaN, AlInN, InGaN / GaN superlattice, InGaN / AlGaN superlattice, InGaN / AlInGaN superlattice, InGaN / AlInN superlattice, GaN / AlGaN superlattice, and GaN / AlInGaN superlattice, and have a thickness of 5 to 1000 nm.
8. The epitaxial structure of a III-nitride semiconductor laser according to claim 1, It is characterized in that The refractive index distribution of the waveguide layer under the first fold steep change has a function y=(e x +e -x ) / (e x -e -x ) curve distribution; the refractive index distribution of the second gradually varying lower waveguide layer has a function y=x -a The third quadrant curve distribution, where a is an odd number greater than 1; The radiation recombination coefficient distribution of the waveguide layer under the first fold abrupt change has a function y=e x / x third quadrant curve distribution; the radiation recombination coefficient distribution of the second gradually varying lower waveguide layer has a function y=x -b The third quadrant curve distribution, where b is an odd number greater than 1; The peak electron drift velocity distribution of the waveguide layer under the first fold abrupt change has a function y=sinx / x 2 The third quadrant curve distribution; the peak electron drift rate distribution of the second gradually changing lower waveguide layer has a function y=x -c The third quadrant curve distribution, where c is an odd number greater than 1; The deformation potential distribution of the first steeply folded lower waveguide layer has a function y=xk / x second three-quadrant curve distribution, where k>0; the deformation potential distribution of the second gradually folded lower waveguide layer has a function y=e x / x 2 The second quadrant curve distribution; The transverse sound velocity distribution of the first steeply folded lower waveguide layer has a function y=xh / x second three-quadrant curve distribution, wherein h>0; the transverse sound velocity distribution of the second gradually folded lower waveguide layer has a function y=xd / x second three-quadrant curve distribution, wherein d>0; The refractive index distribution, radiation recombination coefficient distribution, peak electron drift velocity distribution, and transverse sound velocity distribution of the second gradually varying lower waveguide layer have the following relationship: d≤b≤a≤c.
9. The epitaxial structure of a III-nitride semiconductor laser according to any one of claims 1 to 8, It is characterized in that The active layer is GaN, InGaN, InN, AlInN, AlGaN, AlInGaN, AlN, GaAs, GaP, InP, AlGaAs, AlInGaAs, AlGaInP, InGaAs, InGaA sN, AlInAs, AlInP, AlGaP, InGaP, GaSb, InSb, InAs, InAsSb, AlGaSb, AlSb, InGaSb, AlGaAsSb, InGaAsSb, SiC, Ga 2 O 3 , BN, diamond, any one or any combination thereof, with a thickness of 10 to 100 angstroms, and the barrier layer of the active layer is GaN, InGaN, InN, AlInN, AlGaN, AlInGaN, AlN, GaAs, GaP, InP, AlGaAs, AlInGaAs, AlGaInP, InGaAs, InGaAsN, AlInAs, AlInP, AlGaP, InGaP, GaSb, InSb, InAs, InAsSb, AlGaSb, AlSb, InGaSb, AlGaAsSb, InGaAsSb, SiC, Ga 2 O 3 , BN, diamond, any one or any combination thereof, with a thickness of 10 to 200 angstroms; The lower cladding layer, the lower waveguide layer, the first upper cladding layer, the electron blocking layer, and the second upper cladding layer are GaN, InGaN, InN, AlInN, AlGaN, AlInGaN, AlN, GaAs, GaP, InP, AlGaAs, AlInGaAs, AlGaInP, InGaAs, InGaAsN, AlInAs, AlInP, AlGaP, InGaP, GaSb, InSb, InAs, InAsSb, AlGaSb, AlSb, InGaSb, AlGaAsSb, InGaAsSb, SiC, Ga 2 O 3 , BN, diamond, any one or any combination; The substrate includes sapphire, silicon, Ge, SiC, AlN, GaN, GaAs, InP, InAs, GaSb, sapphire / SiO 2 Composite substrates, Mo, TiW, CuW, Cu, sapphire / AlN composite substrates, diamond, graphene, sapphire / SiNx, sapphire / SiO 2 / SiNx composite substrate, sapphire / SiNx / SiO 2 Composite substrate, magnesium aluminum spinel MgAl 2 O 4 、MgO、ZnO、ZrB 2 、LiAlO 2 and LiGaO 2 Any type of composite substrate.
10. A method for preparing a single crystal thin film of a III-nitride semiconductor laser, specifically The following steps are involved: S1: rotating the substrate 100 in a graphite disk and transferring it into a MOCVD metal organic chemical vapor deposition reaction chamber; S2: Setting the temperature and pressure of the reaction chamber. According to the growth conditions of different layers, the temperature of the reaction chamber is set to 500-1200°C, and the growth pressure in the reaction chamber is controlled to be within the range of 100-550 Torr. S3: Introduce the required reaction gases one by one through the gas flow controller, including TMGa, TEGa, TMAl, TMIn, NH 3 、N 2 and H 2 , control the V / III ratio to 100-80 000 and the ratio of reactive elements; S4: setting the rotation speed of the substrate 100 to 500-1300 rpm; S5: Introduce the required doping elements one by one through the gas flow controller, including Cp 2 Mg、SiH 4 or any of disilane; S6: Control and set different temperatures, pressures, reaction element selection and ratio, rotation speed, growth rate, V / III ratio, and doping element combinations for each layer, and sequentially grow the lower cladding layer 101, the lower waveguide layer 102, the active layer 103, the upper waveguide layer 104, the first upper cladding layer 105, the electron blocking layer 106, and the second upper cladding layer 107; The lower waveguide layer 102 is a refractive index gradient lower waveguide layer 102; the refractive index gradient lower waveguide layer 102 includes a first steeply folded lower waveguide layer 102a and a second gradually folded lower waveguide layer 102b; By controlling the Al / Ga atomic ratio, the injection curve changes to y=g x The curve distribution, where g>1, makes the refractive index distribution of the waveguide layer 102a under the first fold steep change have a function y=(e x +e -x ) / (e x -e -x ) curve distribution; by controlling the In / Ga atomic ratio, the injection curve changes to y = x -a The refractive index distribution of the second gradually varying lower waveguide layer 102b has a function y=x -a (a>1 odd number) The third quadrant curve distribution, where a is an odd number greater than 1; By controlling the Al / Ga atomic ratio, the injection curve changes to y=xe x The curve distribution makes the radiation recombination coefficient distribution of the waveguide layer 102a under the first fold steep change have a function y=e x / x third quadrant curve distribution; by controlling the In / Ga atomic ratio injection change curve is y = x -b The curve distribution makes the radiation recombination coefficient distribution of the second gradually varying lower waveguide layer 102b have a function y=x -b The third quadrant curve distribution, where b is an odd number greater than 1; By controlling the Al / Ga atomic ratio, the injection curve is changed to function y=sinx / x 2 The curve distribution makes the peak electron drift velocity distribution of the waveguide layer 102a under the first fold steep change have the function y=sinx / x 2 The curve distribution of the third quadrant; by controlling the ratio of In / Ga atoms, the injection curve changes to y=x -c The curve distribution makes the peak electron drift velocity distribution of the second gradual lower waveguide layer 102b have a function y=x -c The third quadrant curve distribution, where c is an odd number greater than 1; By controlling the Al / Ga atomic ratio injection change curve to be a function y=xm / x (m>0) curve distribution, the deformation potential distribution of the first fold lower waveguide layer 102a has a function y=xk / x second three-quadrant curve distribution, where k>0; by controlling the In / Ga atomic ratio injection change curve to be y=e x / x curve distribution, so that the deformation potential distribution of the second gradually varying lower waveguide layer 102b has a function y=e x / x 2 The second quadrant curve distribution; By controlling the Al / Ga atomic ratio injection change curve to be a function y=xj / x curve distribution, the lateral sound velocity distribution of the first steeply changing lower waveguide layer 102a has a function y=xh / x second three-quadrant curve distribution, wherein j>0, h>0; by controlling the In / Ga atomic ratio injection change curve to be a function y=arccotx curve distribution, the lateral sound velocity distribution of the second gradually changing lower waveguide layer 102b has a function y=xd / x second three-quadrant curve distribution, wherein d>0.
Citation Information
Cited By
Gallium nitride-based semiconductor laser with divergence angle modulation layer
CN121035773A