Semiconductor structure and forming method thereof
By forming a polysilicon layer, etching silicon nanowires, ion processing and recrystallization in the 3D DRAM silicon column process, the problems of high difficulty in 3D DRAM process and many structural defects are solved, and the product yield is improved.
Patent Information
- Application Number
- CN202310554209.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-15
AI Technical Summary
The process of 3D dynamic random access memory (3D DRAM) silicon column manufacturing process is difficult and easy to develop structural defects, resulting in low product yield.
Silicon nanowires and bitline structures are formed by forming a polysilicon layer on the surface of the bitline material layer, and etching them on the polysilicon layer and bitline material layer. Then, the silicon nanowires are ionized to form an amorphous silicon column, and the recrystallization transformation is performed by ionization. It is a single crystal silicon column, which simplifies the process flow and reduces the probability of structural defects.
This method simplifies the process flow, reduces the probability of structural defects in single crystal silicon columns, improves product yields, and reduces process difficulty.
Smart Images

Figure CN119012684A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of semiconductor technology, and in particular, to a semiconductor structure and a method for forming the same. Background Art
[0002] 3D Dynamic Random Access Memory (3DDRAM) is widely used in mobile devices such as mobile phones and tablet computers due to its advantages such as small size, high integration and fast transmission speed. The silicon pillar manufacturing process of 3DDRAM is difficult and prone to structural defects due to the limitation of the manufacturing process, resulting in low product yield.
[0003] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present disclosure, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention
[0004] In view of this, the present disclosure provides a semiconductor structure and a method for forming the same, which can simplify the process, reduce structural defects, and improve product yield.
[0005] According to one aspect of the present disclosure, there is provided a method for forming a semiconductor structure, comprising:
[0006] providing a substrate, the substrate comprising a bit line material layer;
[0007] forming a polysilicon layer on a surface of the bit line material layer;
[0008] Etching the polysilicon layer and the bit line material layer to form a plurality of silicon nanowires and a bit line structure located below the plurality of silicon nanowires;
[0009] Performing ion treatment on the plurality of silicon nanowires to form a plurality of amorphous silicon pillars;
[0010] The plurality of amorphous silicon pillars are recrystallized to form a plurality of single crystal silicon pillars.
[0011] In an exemplary embodiment of the present disclosure, some of the single crystal silicon pillars in the plurality of single crystal silicon pillars have different crystal orientations.
[0012] In an exemplary embodiment of the present disclosure, a plurality of the silicon nanowires form a plurality of semiconductor column groups spaced apart along a first direction, the semiconductor column groups include a plurality of silicon nanowires spaced apart along a second direction, and a bit line structure is formed under each of the semiconductor column groups; the first direction intersects with the second direction; the polysilicon layer and the bit line material layer are etched to form silicon nanowires and a bit line structure located under the silicon nanowires, including:
[0013] Etching the polysilicon layer and the bit line material layer to form a plurality of first trenches spaced apart along the first direction and extending along the second direction, wherein the first trenches penetrate the polysilicon layer and the bit line material layer;
[0014] forming a first isolation structure in the first trench, wherein the first isolation structure fills the first trench;
[0015] Etching the polysilicon layer and the first isolation structure to form a plurality of second trenches divided along the second direction and extending along the first direction, wherein the second trenches do not penetrate the polysilicon layer, and the second trenches and the first trenches divide the polysilicon layer into a plurality of the silicon nanowires;
[0016] A second isolation structure is formed in the second trench, and the second isolation structure fills up the second trench, wherein the second isolation structure and the remaining first isolation structure together form a shallow trench isolation structure.
[0017] In an exemplary embodiment of the present disclosure, forming the polysilicon layer includes:
[0018] forming a polysilicon material layer on a surface of the bit line material layer;
[0019] Performing thermal annealing on the polysilicon material layer at a first preset temperature and a first preset time to form the polysilicon layer, wherein the unit cell size of the polysilicon layer is in the micrometer order;
[0020] The first preset temperature includes 500° C. to 600° C., and the first preset time includes 2 h to 10 h.
[0021] In an exemplary embodiment of the present disclosure, in a direction perpendicular to the substrate, the height of the silicon nanowire is 80 nm to 150 nm; ion treatment is performed on the silicon nanowire to form an amorphous silicon column, comprising:
[0022] The silicon nanowires are bombarded with ions having a preset energy, wherein the preset energy includes 10keV-100keV.
[0023] In an exemplary embodiment of the present disclosure, the amorphous silicon column is recrystallized to form a single crystal silicon column, comprising:
[0024] Annealing the amorphous silicon column at a second preset temperature and a second preset time to convert the amorphous silicon column into a single crystal silicon column;
[0025] The second preset temperature is 550° C. to 650° C., and the second preset time is 3 h to 8 h.
[0026] According to one aspect of the present disclosure, there is provided 7. a forming method according to any one of the above, wherein the forming method further comprises:
[0027] Etching the shallow trench isolation structure to expose at least a portion of the sidewall of the single crystal silicon column;
[0028] forming a gate oxide layer on the surface of the exposed sidewall of the single crystal silicon column;
[0029] A gate electrode layer is formed on the surface of the gate oxide layer.
[0030] In an exemplary embodiment of the present disclosure, the forming method further includes:
[0031] A passivation layer is formed on the surface of the gate electrode layer, and the passivation layer fills the gap between two adjacent single crystal silicon pillars.
[0032] According to one aspect of the present disclosure, there is provided a semiconductor structure, comprising:
[0033] The bit line structure comprises a bit line material layer and a polysilicon layer located on a surface of the bit line material layer;
[0034] A plurality of single crystal silicon pillars are all located on a surface of the polysilicon layer away from the bit line material layer, and some of the single crystal silicon pillars have different crystal orientations.
[0035] In an exemplary embodiment of the present disclosure, the plurality of single crystal silicon columns form a plurality of single crystal silicon column groups spaced apart along a first direction, the single crystal silicon column groups include a plurality of single crystal silicon columns spaced apart along a second direction, a bit line structure is formed under each of the single crystal silicon column groups, and the first direction intersects with the second direction.
[0036] In an exemplary embodiment of the present disclosure, the semiconductor structure further includes:
[0037] A gate oxide layer, located on the sidewall surface of the single crystal silicon column;
[0038] The gate electrode layer is located on the surface of the gate oxide layer.
[0039] In an exemplary embodiment of the present disclosure, the semiconductor structure further includes:
[0040] The shallow trench isolation structure fills the gap between two adjacent bit line structures and the gap between the single crystal silicon pillars.
[0041] The method for forming a semiconductor structure disclosed in the present invention, on the one hand, can form a polysilicon layer on the surface of a bit line material layer, and in the process of forming silicon nanowires, the bit line material layer and the polysilicon layer can be etched simultaneously to form a bit line structure. In the above process, there is no need to first form silicon nanowires and then bury the bit lines under the silicon nanowires, which helps to reduce the difficulty of the process; on the other hand, since polysilicon cells are usually large, most of the silicon nanowires formed after etching the polysilicon layer are located in the polysilicon cells, and amorphous silicon columns can be obtained after ion treatment of the silicon nanowires. In the process of recrystallizing the amorphous silicon columns, the inside of the amorphous silicon columns will naturally grow epitaxially into single crystal silicon; even if a small number of silicon nanowires are located on the polysilicon grain boundaries, in the process of recrystallization, the grain boundaries will grow along the amorphous silicon columns. In this process, since the lateral size of the amorphous silicon columns is relatively small, the grain boundaries will end at the boundaries of the amorphous silicon columns after growing a very short distance, and the other parts will grow in the form of single crystals, thereby obtaining single crystal silicon columns. In the above process, the probability of structural defects occurring in the single crystal silicon column is low, which helps to improve product yield.
[0042] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.
[0044] Figure 1 Flow chart of a method for forming a semiconductor structure in an embodiment of the present disclosure.
[0045] Figure 2 Schematic diagram of a substrate and a polysilicon layer in an embodiment of the present disclosure.
[0046] Figure 3 It is a top view after completing step S130 in the embodiment of the present disclosure.
[0047] Figure 4 In the embodiment of the present disclosure, the step S130 is completed. Figure 3 Cross-sectional view taken along the aa' direction.
[0048] Figure 5 In the embodiment of the present disclosure, the step S130 is completed. Figure 3 Cross-sectional view taken along the bb' direction.
[0049] Figure 6It is a top view after completing step S310 in the embodiment of the present disclosure.
[0050] Figure 7 It is a top view after completing step S320 in the embodiment of the present disclosure.
[0051] Figure 8 It is a top view after completing step S340 in the embodiment of the present disclosure.
[0052] Fig. 9 In the embodiment of the present disclosure, the step S340 is completed. Figure 8 Cross-sectional view taken along the aa' direction.
[0053] Fig.10 Schematic diagram of an amorphous silicon column in an embodiment of the present disclosure.
[0054] Fig.11 Schematic diagram of a single crystal silicon column in an embodiment of the present disclosure.
[0055] Fig.12 Schematic diagram of a gate trench in an embodiment of the present disclosure.
[0056] Fig.13 Schematic diagram of a gate oxide layer and a gate electrode layer in an embodiment of the present disclosure.
[0057] Fig.14 1 is a top view of the gate oxide layer and the gate electrode layer in the embodiment of the present disclosure.
[0058] Description of reference numerals:
[0059] 1. Substrate; 11. Base; 12. Dielectric layer; 13. Bit line material layer; 2. Polysilicon layer; 21. Silicon nanowire; 22. Amorphous silicon column; 23. Single crystal silicon column; 201. First trench; 202. Second trench; 3. Shallow trench isolation structure; 31. First isolation structure; 32. Second isolation structure; 33. Passivation layer; 301. Gate trench; 100. Bit line structure; 200. Semiconductor column group; 4. Gate oxide layer; 5. Gate electrode layer; x, first direction; y, second direction. DETAILED DESCRIPTION
[0060] Example embodiments will now be described more fully with reference to the accompanying drawings. However, the example embodiments can be implemented in a variety of forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided so that the present disclosure will be comprehensive and complete and fully convey the concepts of the example embodiments to those skilled in the art. The same reference numerals in the figures represent the same or similar structures, and thus their detailed description will be omitted. In addition, the drawings are only schematic illustrations of the present disclosure and are not necessarily drawn to scale.
[0061] Although relative terms such as "upper" and "lower" are used in this specification to describe the relative relationship of one component of the illustration to another component, these terms are used in this specification only for convenience, such as according to the orientation of the examples described in the drawings. It is understood that if the device of the illustration is turned upside down, the component described as "upper" will become the component "lower". When a structure is "on" other structures, it may mean that the structure is formed integrally on the other structure, or that the structure is "directly" disposed on the other structure, or that the structure is "indirectly" disposed on the other structure through another structure.
[0062] The terms "a", "an", "the", "said" and "at least one" are used to indicate the presence of one or more elements / components / etc.; the terms "including" and "having" are used to express an open-ended inclusive meaning and mean that additional elements / components / etc. may exist in addition to the listed elements / components / etc.; the terms "first" and "second" etc. are used merely as labels and are not intended to limit the quantity of their objects.
[0063] In the process of manufacturing vertical nanowire transistors in memory, the following two methods are usually used: 1) In the process of manufacturing 4F2DRAM, silicon nanowires are first formed on a silicon substrate, and then a bit line structure is buried at the bottom of the silicon nanowires. However, the process of burying the bit line structure from above the silicon nanowires is more difficult. 2) In the process of manufacturing 3D DRAM, a multi-layer silicon pillar structure is usually formed on a silicon substrate by epitaxial growth. However, when the number of layers grown is large, the process is more difficult, and the defect density of the formed silicon pillars is getting larger and larger, resulting in a lower product yield.
[0064] Based on this, the present disclosure provides a method for forming a semiconductor structure. Figure 1 A flowchart showing a method for forming a semiconductor structure of the present disclosure is shown in FIG. Figure 1 As shown, the forming method includes steps S110 to S150, wherein:
[0065] Step S110, providing a substrate, wherein the substrate includes a bit line material layer;
[0066] Step S120, forming a polysilicon layer on the surface of the bit line material layer;
[0067] Step S130, etching the polysilicon layer and the bit line material layer to form a plurality of silicon nanowires and a bit line structure located below the plurality of silicon nanowires;
[0068] Step S140, performing ion treatment on the plurality of silicon nanowires to form a plurality of amorphous silicon pillars;
[0069] Step S150, recrystallizing the plurality of amorphous silicon pillars to form a plurality of single crystal silicon pillars.
[0070] The method for forming a semiconductor structure disclosed in the present invention, on the one hand, can form a polysilicon layer on the surface of a bit line material layer, and in the process of forming silicon nanowires, the bit line material layer and the polysilicon layer can be etched simultaneously to form a bit line structure. In the above process, there is no need to first form silicon nanowires and then bury the bit lines under the silicon nanowires, which helps to reduce the process difficulty; on the other hand, since the polysilicon cell is usually large, most of the silicon nanowires formed after etching the polysilicon layer are located in the polysilicon cell, and amorphous silicon columns can be obtained after ion treatment of the silicon nanowires. In the process of recrystallizing the amorphous silicon column, the amorphous silicon column can be formed into a single crystal silicon column on the polysilicon cell by, for example, low-temperature solid phase epitaxy; even if a small part of the silicon nanowires is located on the polysilicon grain boundary, during the recrystallization process, the grain boundary will grow along the amorphous silicon column. In this process, since the lateral size of the amorphous silicon column is relatively small, the grain boundary will end at the boundary of the amorphous silicon column after growing a very short distance, and the other part will grow in the form of a single crystal, thereby obtaining a single crystal silicon column. In the above process, the probability of structural defects occurring in the single crystal silicon column is low, which helps to improve product yield.
[0071] The steps and specific details of the method for forming a semiconductor structure disclosed in the present invention are described in detail below:
[0072] like Figure 1 As shown, in step S110, a substrate is provided, wherein the substrate includes a bit line material layer.
[0073] In some embodiments of the present disclosure, Figure 2 As shown, the substrate 1 may include a base 11, a dielectric layer 12 and a bit line material layer 13, wherein: the base 11 may be a flat plate structure, which may be rectangular, circular, elliptical, polygonal or irregular in shape, and the base 11 may be a carrier, a wafer or a structure after any process in the semiconductor manufacturing process, and the shape and material of the base 11 are not specifically limited here. The dielectric layer 12 may cover the surface of the base 11, and the material of the dielectric layer 12 may be an insulating material, for example, the material may be silicon oxide. The dielectric layer 12 may be formed on the surface of the base 11 by chemical vapor deposition, physical vapor deposition or atomic layer deposition. The bit line material layer 13 is located on the surface of the dielectric layer 12, and it can be used to form a bit line structure. The material of the bit line material layer 13 may be a conductive material, for example, the material may include titanium nitride and / or tungsten. The bit line material layer 13 can be formed on the surface of the dielectric layer 12 by chemical vapor deposition, physical vapor deposition or atomic layer deposition. Of course, the bit line material layer 13 can also be formed by other methods. The formation method of the bit line material layer 13 is not particularly limited here.
[0074] like Figure 1As shown, in step S120 , a polysilicon layer 2 is formed on the surface of the bit line material layer 13 .
[0075] Please continue to see Figure 2 As shown, the polysilicon layer 2 can be a thin film covering the surface of the bit line material layer 13, or a coating covering the surface of the bit line material layer 13. The specific form of the polysilicon layer 2 is not particularly limited here. The polysilicon layer 2 can be formed on the surface of the bit line material layer 13 by chemical vapor deposition, physical vapor deposition or atomic layer deposition. Of course, the polysilicon layer 2 can also be formed by other methods. The formation method of the polysilicon layer 2 is not particularly limited here. In some embodiments of the present disclosure, the thickness of the polysilicon layer 2 can be 100nm to 200nm. For example, its thickness can be 100nm, 120nm, 140nm, 160nm, 180nm or 200nm. Of course, it can also be other thicknesses, which are not listed here.
[0076] In an exemplary embodiment of the present disclosure, forming the polysilicon layer 2 may include steps S210 and S220, wherein:
[0077] Step S210 , forming a polysilicon material layer on the surface of the bit line material layer 13 .
[0078] The material of the polysilicon material layer can be polysilicon, and polysilicon can be deposited on the surface of the bit line material layer 13 by chemical vapor deposition, physical vapor deposition or atomic layer deposition to form a polysilicon material layer. Of course, the polysilicon material layer can also be formed by other methods, and the formation method of the polysilicon material layer is not specifically limited here.
[0079] Step S220 , thermally annealing the polysilicon material layer at a first preset temperature and a first preset time to form the polysilicon layer 2 , wherein the unit cell size of the polysilicon layer 2 is in the micrometer order.
[0080] The size of the unit cells in the polysilicon material layer can be controlled by thermal annealing. For example, the polysilicon material layer can be thermally annealed at a first preset temperature and a first preset time so that the unit cells in the polysilicon material layer grow to the micrometer level. The first preset temperature may include 500°C to 600°C, for example, it may be 500°C, 520°C, 540°C, 560°C, 580°C or 600°C. Of course, it can also be other temperatures, which are not listed here. The first preset time may include 2h to 10h, for example, it can be 2h, 4h, 6h, 8h or 10h. Of course, it can also be other times, which are not listed here. It should be noted that the polysilicon material layer after thermal annealing can be used as the polysilicon layer 2.
[0081] like Figure 1As shown, in step S130 , the polysilicon layer 2 and the bit line material layer 13 are etched to form a plurality of silicon nanowires 21 and a bit line structure 100 located below the plurality of silicon nanowires 21 .
[0082] like Figure 3-Figure 5 As shown, the polysilicon layer 2 and the bit line material layer 13 located below the polysilicon layer 2 can be etched by a dry etching process, thereby forming a plurality of silicon nanowires 21 distributed in an array in the polysilicon layer 2. In this process, a bit line structure 100 located below the silicon nanowires 21 can also be formed simultaneously. For example, a plurality of silicon nanowires 21 can form a plurality of semiconductor column groups 200 spaced apart along a first direction x, each semiconductor column group 200 can include a plurality of silicon nanowires 21 spaced apart along a second direction y, and a bit line structure 100 is formed below each semiconductor column group 200. The first direction x intersects with the second direction y, for example, the first direction x and the second direction y can be perpendicular to each other. It should be noted that verticality can be absolutely vertical or approximately vertical, and there will inevitably be deviations during the manufacturing process. In the present disclosure, the angle deviation may be caused by the manufacturing process limitation, so that the angle between the first direction x and the second direction y has a certain deviation. As long as the angle deviation between the first direction x and the second direction y is within a preset range, the first direction x can be considered to be perpendicular to the second direction y. For example, the preset range may be 10°, that is, when the angle between the first direction x and the second direction y is greater than or equal to 80° and less than or equal to 100°, the first direction x and the second direction y may be considered to be perpendicular.
[0083] In an exemplary embodiment of the present disclosure, etching the polysilicon layer 2 and the bit line material layer 13 to form the silicon nanowire 21 and the bit line structure 100 located below the silicon nanowire 21 (i.e., step S130) may include steps S310 to S340, wherein:
[0084] Step S310 , etching the polysilicon layer 2 and the bit line material layer 13 to form a plurality of first trenches 201 spaced apart along the first direction x and extending along the second direction y, wherein the first trenches 201 penetrate the polysilicon layer 2 and the bit line material layer 13 .
[0085] like Figure 6 As shown, a dry etching process can be used to etch the polysilicon layer 2 and the bit line material layer 13, thereby forming a plurality of first grooves 201 spaced apart along the first direction x, and the etching gas can be a mixture of chlorine and argon. The first grooves 201 can be strip-shaped and can extend along the second direction y. In a direction perpendicular to the substrate 1, the first grooves 201 can penetrate the polysilicon layer 2 and the bit line material layer 13; in the second direction y, the first grooves 201 can penetrate the polysilicon layer 2 and the bit line material layer 13 at the same time.
[0086] Step S320 , forming a first isolation structure 31 in the first trench 201 , wherein the first isolation structure 31 fills up the first trench 201 .
[0087] like Figure 7 As shown, the material of the first isolation structure 31 may be an insulating material, for example, the material may be silicon oxide. The insulating material may be filled in the first trench 201 by chemical vapor deposition, physical vapor deposition, or atomic layer deposition, thereby forming the first isolation structure 31 in the first trench 201. Of course, the first isolation structure 31 may also be formed by other methods, and the formation method of the first isolation structure 31 is not particularly limited here. In some embodiments of the present disclosure, the first isolation structure 31 may fill the first trench 201, and its top surface may be flush with the top surface of the polysilicon layer 2.
[0088] In the process of forming the first isolation structure 31, for the convenience of process, insulating material can be deposited on the surface of the polysilicon layer 2 until the insulating material fills each first groove 201 and then stops depositing. Subsequently, the insulating material can be planarized to remove the insulating material on the surface of the polysilicon layer 2, and the surface of the insulating material in the first groove 201 is made flush with the surface of the polysilicon layer 2. The insulating material remaining in the first groove 201 after the planarization process can be used as the first isolation structure 31.
[0089] In step S330, the polysilicon layer 2 and the first isolation structure 31 are etched to form a plurality of second grooves 202 divided along the second direction y and extending along the first direction x, wherein the second grooves 202 do not penetrate the polysilicon layer 2, and the second grooves 202 and the first grooves 201 divide the polysilicon layer 2 into a plurality of silicon nanowires 21.
[0090] Please continue to see Figure 3 As shown, the structure formed by the polysilicon layer 2 and the first isolation structure 31 can be etched by a dry etching process, thereby forming a plurality of second grooves 202 spaced apart along the second direction y, and the etching gas for dry etching can be a mixture of chlorine and argon. The second groove 202 can be in a strip shape and can extend along the first direction x. In the first direction x, the second groove 202 can penetrate both ends of the polysilicon layer 2; in the direction perpendicular to the substrate 1, the second groove 202 does not penetrate the polysilicon layer 2, that is, compared with the first groove 201, the depth of the second groove 202 is relatively shallow, and the bottom of the second groove 202 still retains the polysilicon layer 2. The second groove 202 intersects with the first groove 201, and the polysilicon layer 2 can be separated into a plurality of silicon nanowires 21 distributed in an array by the second groove 202 and the first groove 201. In the direction parallel to the substrate 1, the cross section of the silicon nanowire 21 can be rectangular.
[0091] In some embodiments of the present disclosure, in the direction perpendicular to the substrate 1, the thickness of the polysilicon layer 2 remaining at the bottom of the second trench 202 may be 20nm to 50nm, for example, its thickness may be 20nm, 30nm, 40nm or 50nm, of course, it may be other thicknesses, which are not listed here. In some embodiments of the present disclosure, in the direction perpendicular to the substrate 1, the height of the silicon nanowire 21 may be 80nm to 150nm, for example, its height may be 80nm, 100nm, 120nm, 140nm or 150nm, and in the direction parallel to the substrate 1, the lateral dimension of the silicon nanowire 21 is less than 10nm, of course, the silicon nanowire 21 may also be other dimensions, which are not listed here.
[0092] It should be noted that the portion above the bottom of the second trench 202 in the polysilicon layer 2 can be used as the silicon nanowire 21, and the portion below the bottom of the second trench 202 can be used as a part of the bit line structure 100, that is, the bit line structure 100 can include the polysilicon layer 2 below the semiconductor column group 200 composed of the silicon nanowire 21 and the bit line material layer 13 directly below the polysilicon layer 2. Since the first trench 201 divides the bit line material layer 13 and the polysilicon layer 2 into a plurality of strip structures, a bit line structure 100 can be formed under each semiconductor column group 200. At the same time, since the first isolation structure 31 fills the first trench 201 used to divide the bit line material layer 13 and the polysilicon layer 2, the adjacent bit line structures 100 can be insulated and isolated by the first isolation structure 31, which can reduce the risk of short circuit and improve the product yield.
[0093] Step S340 , forming a second isolation structure 32 in the second trench 202 , wherein the second isolation structure 32 fills up the second trench 202 , wherein the second isolation structure 32 and the remaining first isolation structure 31 together form a shallow trench isolation structure 3 .
[0094] like Figure 8 and Fig. 9 As shown, the material of the second isolation structure 32 can be the same as that of the first isolation structure 31. For example, the material of the second isolation structure 32 and the material of the first isolation structure 31 can both be insulating materials. For example, the material of the second isolation structure 32 and the material of the first isolation structure 31 can both be silicon oxide. The insulating material can be filled in the second trench 202 by chemical vapor deposition, physical vapor deposition, or atomic layer deposition, thereby forming the second isolation structure 32 in the second trench 202. Of course, the second isolation structure 32 can also be formed by other methods. The formation method of the second isolation structure 32 is not particularly limited here. In some embodiments of the present disclosure, such as Fig. 9As shown, the second isolation structure 32 may fill up the second trench 202 , and its top surface may be flush with the top surface of the polysilicon layer 2 .
[0095] In the process of forming the first isolation structure 31, for the convenience of process, insulating material can be deposited on the surface of the structure jointly formed by the polysilicon layer 2 and the first isolation structure 31 until the insulating material fills each second groove 202 and the deposition is stopped. Subsequently, the insulating material can be planarized to remove the insulating material located on the surface of the polysilicon layer 2 and the first isolation structure 31, and the surface of the insulating material located in the second groove 202 is made flush with the surface of the polysilicon layer 2. The insulating material remaining in the second groove 202 after the planarization process can be used as the second isolation structure 32.
[0096] like Figure 1 As shown, in step S140 , ion treatment is performed on the plurality of silicon nanowires 21 to form a plurality of amorphous silicon pillars 22 .
[0097] like Fig.10 As shown, the silicon nanowire 21 can be ion-treated by ion bombardment, thereby converting the silicon nanowire 21 into an amorphous silicon pillar 22. For example, the silicon nanowire 21 can be bombarded with ions having a preset energy, and the ions can be silicon ions, germanium ions, or arsenic ions. The preset energy can include 10keV to 100keV, for example, it can be 10keV, 30keV, 50keV, 70keV, 90keV, or 100keV. Of course, it can also be other energies, which are not listed here one by one. It should be noted that multiple silicon nanowires 21 can be ion-treated at the same time, thereby forming multiple amorphous silicon pillars 22 at the same time.
[0098] like Figure 1 As shown, in step S150 , the plurality of amorphous silicon pillars 22 are recrystallized to form a plurality of single crystal silicon pillars 23 .
[0099] like Fig.11As shown, in some embodiments of the present disclosure, the amorphous silicon column 22 can be recrystallized by low-temperature solid phase epitaxy, and then converted into a single crystal silicon column 23. During the recrystallization process, since the polycrystalline silicon cell is usually large, most of the silicon nanowires 21 formed after etching the polycrystalline silicon layer 2 are located in the polycrystalline silicon cell. After ion treatment of the silicon nanowires 21, the amorphous silicon column 22 can be obtained. During the recrystallization process of the amorphous silicon column 22, the inside of the amorphous silicon column 22 will naturally grow epitaxially into single crystal silicon; even if a small part of the silicon nanowires 21 will be located on the polycrystalline silicon grain boundary, during the recrystallization process, the grain boundary will grow along the amorphous silicon column 22. In this process, since the lateral size of the amorphous silicon column 22 is relatively small, the grain boundary will end at the boundary of the amorphous silicon column 22 after growing a short distance, and the other parts will grow in the form of a single crystal, thereby obtaining a single crystal silicon column 23. In the above process, the probability of structural defects in the single crystal silicon column 23 is low, which helps to improve the product yield.
[0100] In an exemplary embodiment of the present disclosure, the amorphous silicon column 22 may be annealed at a second preset temperature and a second preset time, thereby converting the amorphous silicon column 22 into a single crystal silicon column 23. The second preset temperature may include 550°C to 650°C, for example, it may be 550°C, 570°C, 590°C, 610°C, 630°C or 650°C. Of course, it may be other temperatures, which are not listed here. The second preset time may include 3h to 8h (h represents hours), for example, it may be 3h, 4h, 5h, 6h, 7h or 8h. Of course, it may be other durations, which are not listed here. It should be noted that the amorphous silicon columns 22 after annealing are basically converted into single crystal silicon columns 23.
[0101] In an exemplary embodiment of the present disclosure, a plurality of amorphous silicon columns 22 may be recrystallized at the same time, thereby simultaneously forming a plurality of single crystal silicon columns 23. It should be noted that some of the single crystal silicon columns 23 have different crystal orientations among the plurality of single crystal silicon columns 23. For example, 2 is a seed layer, and since the polycrystalline silicon layer 2 directly below the plurality of amorphous silicon columns 22 may come from different unit cells, and the crystal orientations of different unit cells may be different, the single crystal silicon columns 23 grown based on different unit cells have different crystal orientations. For example, if a plurality of single crystal silicon columns 23 are grown based on unit cells with two different crystal orientations, the plurality of single crystal silicon columns 23 may include at least two single crystal silicon columns 23 with different crystal orientations; if a plurality of single crystal silicon columns 23 are grown based on unit cells with three different crystal orientations, the plurality of single crystal silicon columns 23 may include at least three single crystal silicon columns 23 with different crystal orientations; if a plurality of single crystal silicon columns 23 are grown based on unit cells with four different crystal orientations, the plurality of single crystal silicon columns 23 may include at least four single crystal silicon columns 23 with different crystal orientations, and so on.
[0102] In an exemplary embodiment of the present disclosure, the method for forming a semiconductor structure of the present disclosure may further include steps S160 to S180, wherein:
[0103] Step S160 , etching the shallow trench isolation structure 3 to expose at least a portion of the sidewall of the single crystal silicon pillar 23 .
[0104] like Fig.12 As shown, after the single crystal silicon pillar 23 is formed, the first isolation structure 31 and / or the second isolation structure 32 may be etched by a dry etching process or a wet etching process, thereby forming a gate trench 301 that exposes at least a portion of the sidewall of the single crystal silicon pillar 23, so as to facilitate the subsequent formation of a gate oxide layer 4 on the sidewall surface of the single crystal silicon pillar 23. For example, the gate trench 301 formed after the first isolation structure 31 and / or the second isolation structure 32 are etched back may expose the sidewall of the upper half of each single crystal silicon pillar 23; or, the gate trench 301 formed after the first isolation structure 31 and / or the second isolation structure 32 are etched back may expose the entire sidewall of the single crystal silicon pillar 23.
[0105] It should be noted that the etching gas or etching solution can be selected according to the specific material of the first isolation structure 31 and / or the second isolation structure 32, as long as the etching solution or etching gas can etch away the first isolation structure 31 and / or the second isolation structure 32 without damaging the single crystal silicon column 23.
[0106] Step S170 , forming a gate oxide layer 4 on the surface of the exposed sidewall of the single crystal silicon pillar 23 .
[0107] like Fig.13 As shown, the material of the gate oxide layer 4 may be silicon oxide, and the gate oxide layer 4 may be formed on the surface of the side wall exposed in the single crystal silicon column 23 by thermal oxidation, in-situ water vapor oxidation or atomic layer deposition. Of course, the gate oxide layer 4 may also be formed by other methods, and the formation method of the gate oxide layer 4 is not particularly limited here. The gate oxide layer 4 may cover a portion of the surface of the side wall exposed in the single crystal silicon column 23. For example, when the cross section of the single crystal silicon column 23 is rectangular, the gate oxide layer 4 may cover the surface of one side wall of the single crystal silicon column 23; or, the gate oxide layer 4 may cover the surface of two oppositely distributed side walls in the single crystal silicon column 23; or, the gate oxide layer 4 may cover the side wall of the single crystal silicon column 23.
[0108] Step S180 , forming a gate electrode layer 5 on the surface of the gate oxide layer 4 .
[0109] Please continue to see Fig.13As shown, the material of the gate electrode layer 5 may be a conductive material, for example, it may include titanium nitride, tungsten or polysilicon. The gate electrode layer 5 may be formed on the surface of the gate oxide layer 4 by chemical vapor deposition, physical vapor deposition or atomic layer deposition. Of course, the gate electrode layer 5 may also be formed by other methods, and the formation method of the gate electrode layer 5 is not particularly limited here. In some embodiments of the present disclosure, when the cross-section of the single crystal silicon column 23 is rectangular and the gate oxide layer 4 covers the surfaces of two oppositely distributed side walls in the single crystal silicon column 23, the gate electrode layer 5 may respectively cover the surfaces of the two gate oxide layers 4, thereby forming a dual-gate structure; or, as Fig.14 As shown, when the gate oxide layer 4 covers the sidewall of the single crystal silicon pillar 23, the gate electrode layer 5 can extend along the first direction x and cover the outer periphery of each single crystal silicon pillar 23 distributed along the first direction x, thereby forming a full-ring gate structure.
[0110] In an exemplary embodiment of the present disclosure, the method for forming a semiconductor structure of the present disclosure may further include:
[0111] Step S190 , forming a passivation layer 33 on the surface of the gate electrode layer 5 , wherein the passivation layer 33 fills the gap between two adjacent single crystal silicon pillars 23 .
[0112] Please continue to see Fig.13 As shown, after forming the gate electrode layer 5, a passivation layer 33 can be formed on the top of the gate electrode layer 5. The material of the passivation layer 33 is the same as that of the first isolation structure 31 and the second isolation structure 32. For example, the materials of the passivation layer 33, the first isolation structure 31 and the second isolation structure 32 can all be silicon oxide. The surface of the gate electrode layer 5 can be insulated and isolated by the passivation layer 33, which can help reduce the risk of short circuit between the gate electrode layer 5 and other structures formed subsequently, thereby improving the product yield. The first isolation structure 31, the second isolation structure 32 and the passivation layer 33 can together constitute a shallow trench isolation structure 3.
[0113] In some embodiments of the present disclosure, the semiconductor structure formed by the method for forming a semiconductor structure of the present disclosure may be a 4F2 DRAM. In the 4F2 DRAM manufacturing process, a bit line material layer 13 may be deposited first, and then a polysilicon layer 2 may be formed on the surface of the bit line material layer 13 by deposition, and the polysilicon layer 2 may be processed to obtain a vertical single crystal silicon column 23. The manufacturing process is less difficult and has a lower probability of defects. In other embodiments of the present disclosure, a multi-layer stacked semiconductor structure may be formed by the method for forming a semiconductor structure of the present disclosure to obtain a high-density 3D DRAM.
[0114] It should be noted that, although the steps of the method for forming a semiconductor structure in the present disclosure are described in a specific order in the accompanying drawings, this does not require or imply that the steps must be performed in this specific order, or that all the steps shown must be performed to achieve the desired results. Additionally or alternatively, some steps may be omitted, multiple steps may be combined into one step, and / or one step may be decomposed into multiple steps, etc.
[0115] The present disclosure also provides a semiconductor structure, which is formed by the method for forming a semiconductor structure in any of the above embodiments. Fig.13 and Fig.14 As shown, the semiconductor structure includes a bit line structure 100 and a plurality of single crystal silicon pillars 23, wherein:
[0116] The bit line structure 100 includes a bit line material layer 13 and a polysilicon layer 2 located on the surface of the bit line material layer 13;
[0117] The plurality of single crystal silicon pillars 23 are all located on the surface of the polysilicon layer 2 away from the bit line material layer 13 , and some of the single crystal silicon pillars 23 have different crystal orientations.
[0118] In some embodiments of the present disclosure, the bit line structure 100 may be located on a substrate, which may include a base 11 and a dielectric layer 12, wherein: the base 11 may be a flat plate structure, which may be rectangular, circular, elliptical, polygonal or irregular in shape, and the base 11 may be a carrier, a wafer or a structure after any process in the semiconductor manufacturing process, and the shape and material of the base 11 are not specifically limited. The dielectric layer 12 may cover the surface of the base 11, and the material of the dielectric layer 12 may be an insulating material, for example, the material may be silicon oxide.
[0119] The bit line structure 100 may be in a strip shape and may extend along the second direction y. There may be a plurality of bit line structures 100, and the plurality of bit line structures 100 may be spaced apart along the first direction x. The bit line structure 100 may include a bit line material layer 13 and a polysilicon layer 2 located on the surface of the bit line material layer 13, wherein the material of the bit line material layer 13 may be a conductive material, for example, the material may include titanium nitride and / or tungsten, etc.; the material of the polysilicon layer 2 may be polysilicon.
[0120] The plurality of single crystal silicon pillars 23 may form a plurality of groups of single crystal silicon pillars 23 spaced apart along the first direction x, each group of single crystal silicon pillars 23 may include a plurality of single crystal silicon pillars 23 spaced apart along the second direction y, a bit line structure 100 is provided below each group of single crystal silicon pillars 23, and some of the single crystal silicon pillars 23 in the plurality of single crystal silicon pillars 23 have different crystal orientations. For example, the amorphous silicon pillar 22 is recrystallized using the polycrystalline silicon layer 2 directly below it as a seed layer, and since the polycrystalline silicon layer 2 directly below the plurality of amorphous silicon pillars 22 may come from different unit cells, and the crystal orientations of different unit cells may be different, the single crystal silicon pillars 23 grown based on different unit cells have different crystal orientations. For example, if a plurality of single crystal silicon columns 23 are grown based on unit cells with two different crystal orientations, the plurality of single crystal silicon columns 23 may include at least two single crystal silicon columns 23 with different crystal orientations; if a plurality of single crystal silicon columns 23 are grown based on unit cells with three different crystal orientations, the plurality of single crystal silicon columns 23 may include at least three single crystal silicon columns 23 with different crystal orientations; if a plurality of single crystal silicon columns 23 are grown based on unit cells with four different crystal orientations, the plurality of single crystal silicon columns 23 may include at least four single crystal silicon columns 23 with different crystal orientations, and so on.
[0121] In an exemplary embodiment of the present disclosure, the semiconductor structure of the present disclosure may further include a gate oxide layer 4 and a gate electrode layer 5, wherein:
[0122] The material of the gate oxide layer 4 may be silicon oxide, which may be located on the sidewall surface of the single crystal silicon column 23. For example, the gate oxide layer 4 may cover a portion of the sidewall surface of the single crystal silicon column 23. For example, when the cross section of the single crystal silicon column 23 is rectangular, the gate oxide layer 4 may cover the surface of one sidewall of the single crystal silicon column 23; or, the gate oxide layer 4 may cover the surfaces of two oppositely distributed sidewalls of the single crystal silicon column 23; or, the gate oxide layer 4 may cover the sidewall of the single crystal silicon column 23 all around.
[0123] The gate electrode layer 5 is located on the surface of the gate oxide layer 4. The material of the gate electrode layer 5 may be a conductive material, for example, it may include titanium nitride, tungsten or polysilicon. In some embodiments of the present disclosure, when the cross-section of the single crystal silicon column 23 is rectangular and the gate oxide layer 4 covers the surfaces of two oppositely distributed side walls in the single crystal silicon column 23, the gate electrode layer 5 may cover the surfaces of the two gate oxide layers 4 respectively, thereby forming a double-gate structure; or, when the gate oxide layer 4 covers the side wall of the single crystal silicon column 23 for one circle, the gate electrode layer 5 may extend along the first direction x and cover the periphery of each single crystal silicon column 23 distributed along the first direction x, thereby forming a full-ring gate structure.
[0124] In some embodiments of the present disclosure, the semiconductor structure of the present disclosure may further include a shallow trench isolation structure 3, and the material of the shallow trench isolation structure 3 may be an insulating material, for example, the material may be silicon oxide. The shallow trench isolation structure 3 may fill the gap between two adjacent bit line structures 100, and the gap between each single crystal silicon column 23. The adjacent bit line structures 100 may be insulated and isolated by the shallow trench isolation structure 3, and at the same time, the gate electrode layers 5 on different single crystal silicon columns 23 may also be insulated and isolated by the shallow trench isolation structure 3, which may reduce the probability of coupling or short circuit between different gate electrode layers 5, and may also reduce the probability of coupling or short circuit between the gate electrode layer 5 and other structures formed subsequently, which helps to improve the product yield.
[0125] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the invention disclosed herein. The present disclosure is intended to cover any variations, uses or adaptations of the present disclosure, which follow the general principles of the present disclosure and include common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The description and examples are intended to be exemplary only, and the true scope and spirit of the present disclosure are indicated by the appended claims.
Claims
1. A method for forming a semiconductor structure, It is characterized in that include: providing a substrate, the substrate comprising a bit line material layer; forming a polysilicon layer on a surface of the bit line material layer; Etching the polysilicon layer and the bit line material layer to form a plurality of silicon nanowires and a bit line structure located below the plurality of silicon nanowires; Performing ion treatment on the plurality of silicon nanowires to form a plurality of amorphous silicon pillars; The plurality of amorphous silicon pillars are recrystallized to form a plurality of single crystal silicon pillars.
2. The forming method according to claim 1, It is characterized in that Some of the single crystal silicon columns among the plurality of single crystal silicon columns have different crystal orientations.
3. The forming method according to claim 1, It is characterized in that The plurality of silicon nanowires form a plurality of semiconductor column groups spaced apart along a first direction, the semiconductor column groups include a plurality of silicon nanowires spaced apart along a second direction, and a bit line structure is formed under each semiconductor column group; the first direction intersects the second direction; The polysilicon layer and the bit line material layer are etched to form a silicon nanowire and a bit line structure located below the silicon nanowire, comprising: Etching the polysilicon layer and the bit line material layer to form a plurality of first trenches spaced apart along the first direction and extending along the second direction, wherein the first trenches penetrate the polysilicon layer and the bit line material layer; forming a first isolation structure in the first trench, wherein the first isolation structure fills the first trench; Etching the polysilicon layer and the first isolation structure to form a plurality of second trenches divided along the second direction and extending along the first direction, wherein the second trenches do not penetrate the polysilicon layer, and the second trenches and the first trenches divide the polysilicon layer into a plurality of the silicon nanowires; A second isolation structure is formed in the second trench, and the second isolation structure fills up the second trench, wherein the second isolation structure and the remaining first isolation structure together form a shallow trench isolation structure.
4. The forming method according to any one of claims 1 to 3, It is characterized in that Forming the polysilicon layer comprises: forming a polysilicon material layer on a surface of the bit line material layer; Performing thermal annealing on the polysilicon material layer at a first preset temperature and a first preset time to form the polysilicon layer, wherein the unit cell size of the polysilicon layer is in the micrometer order; The first preset temperature includes 500° C. to 600° C., and the first preset time includes 2 h to 10 h.
5. The forming method according to any one of claims 1 to 3, It is characterized in that In a direction perpendicular to the substrate, the height of the silicon nanowire is 80nm to 150nm; and the silicon nanowire is ion treated to form an amorphous silicon column, comprising: The silicon nanowires are bombarded with ions having a preset energy, wherein the preset energy includes 10keV to 100keV.
6. The forming method according to any one of claims 1 to 3, It is characterized in that Recrystallizing the amorphous silicon column to form a single crystal silicon column, comprising: Annealing the amorphous silicon column at a second preset temperature and a second preset time to convert the amorphous silicon column into a single crystal silicon column; The second preset temperature is 550° C. to 650° C., and the second preset time is 3 h to 8 h.
7. The forming method according to claim 3, It is characterized in that The forming method further comprises: Etching the shallow trench isolation structure to expose at least a portion of the sidewall of the single crystal silicon column; forming a gate oxide layer on the surface of the exposed sidewall of the single crystal silicon column; A gate electrode layer is formed on the surface of the gate oxide layer.
8. The forming method according to claim 7, It is characterized in that The forming method further comprises: A passivation layer is formed on the surface of the gate electrode layer, and the passivation layer fills the gap between two adjacent single crystal silicon pillars.
9. A semiconductor structure, It is characterized in that include: The bit line structure comprises a bit line material layer and a polysilicon layer located on a surface of the bit line material layer; A plurality of single crystal silicon pillars are all located on a surface of the polysilicon layer away from the bit line material layer, and some of the single crystal silicon pillars have different crystal orientations.
10. The semiconductor structure according to claim 9, It is characterized in that The plurality of single crystal silicon columns form a plurality of single crystal silicon column groups spaced apart along a first direction, the single crystal silicon column groups include a plurality of single crystal silicon columns spaced apart along a second direction, a bit line structure is formed under each of the single crystal silicon column groups, and the first direction intersects with the second direction.
11. The semiconductor structure according to claim 9, It is characterized in that The semiconductor structure further comprises: A gate oxide layer, located on the sidewall surface of the single crystal silicon column; The gate electrode layer is located on the surface of the gate oxide layer.
12. The semiconductor structure according to claim 9, It is characterized in that The semiconductor structure further comprises: The shallow trench isolation structure fills the gap between two adjacent bit line structures and the gap between the single crystal silicon pillars.
Citation Information
Patent Citations
Manufacturing method of semiconductor structure and semiconductor structure
CN114141712A
Semiconductor structure and manufacturing method thereof
CN115249662A
Semiconductor structure and method for manufacturing same
US20220028730A1
Method of fabricating a capacitor under bit line structure with increased capacitance without increasing the aspect ratio for a dry etched bit line contact hole