Gallium-containing bismuth telluride-based thermoelectric material and preparation method thereof
By doping gallium near the grain boundaries with gallium-containing bismuth telluride-based thermoelectric materials, the challenges of carrier and phonon transport have been solved, enabling the preparation of high-performance and stable thermoelectric materials suitable for large-scale industrial production.
Patent Information
- Application Number
- CN202411101981.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
Existing thermoelectric materials face challenges in carrier and phonon transport, structural defects affect performance, and they are difficult to apply in large-scale industrial production.
By using gallium-containing bismuth telluride-based thermoelectric materials, gallium is doped near the grain boundaries. The transport of charge carriers and phonons is synergistically controlled by the nanoscale second phase of gallium and the anomalous solidification strategy. Combined with vacuum discharge plasma sintering and hot deformation treatment, materials with high microhardness and high structural stability are prepared.
It improves thermoelectric performance, reduces lattice thermal conductivity, optimizes carrier mobility, is suitable for large-scale industrial production, and has high microhardness and structural stability.
Smart Images

Figure CN119012893A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of energy conversion technology, and more specifically, to a gallium-containing bismuth telluride-based thermoelectric material and a preparation method thereof. Background Art
[0002] With the development of energy science, environmental problems are becoming increasingly prominent, and it is urgent to find new energy technologies. Thermoelectric materials based on the Seebeck effect and the Peltier effect can directly realize the mutual conversion between thermal energy and electrical energy, and the prepared thermoelectric devices can be directly applied to the fields of power generation and refrigeration. The dimensionless thermoelectric figure of merit zT is a standard for measuring the performance of thermoelectric materials (zT = σα 2 T / κ, where σ is the electrical conductivity, α is the Seebeck coefficient, and κ is the thermal conductivity (including the carrier thermal conductivity κ e and lattice thermal conductivity κ L ), T is temperature in K). Excellent thermoelectric materials require high Seebeck coefficient, high electrical conductivity and low thermal conductivity. Excellent thermoelectric devices not only require high zT, but also long-term stability of the device. In order to obtain excellent zT values, thermoelectric materials should have a high Seebeck coefficient α similar to ceramics, a high electrical conductivity σ similar to metals, and an ultra-low lattice thermal conductivity κ similar to glass. L . This combination embodies the "electronic crystal-phonon glass" paradigm proposed by Slack. However, the inherent connection between carriers and phonons due to the periodic potential field of the lattice poses a challenge to this paradigm. In addition, structural defects such as 0D point defects, 1D dislocations, 2D grain boundaries and 3D nanoprecipitates can destroy the periodicity of the lattice and hinder the transport of phonons and electrons. In contrast, enhancing the texture or grain size can simultaneously improve the carrier mobility μ and the lattice thermal conductivity κ L Therefore, rational microstructure design and engineering become crucial to enhance phonon scattering and facilitate carrier transport.
[0003] In this context, grain boundaries provide a rich research area for improving thermoelectric performance due to their complex microstructure and different chemical composition relative to adjacent grains. By changing these properties of grain boundaries, which is called grain boundary engineering, the transport of carriers and phonons can be simultaneously regulated. On the one hand, grain boundary engineering is an effective strategy to enhance phonon scattering at grain boundaries, significantly reducing the lattice thermal conductivity κ L On the other hand, grain boundary engineering can optimize electrical transport properties, such as increasing carrier mobility μ by reducing grain boundary resistance, or improving Seebeck coefficient α by energy filtering effect. In addition, impurity elements tend to accumulate at grain boundaries due to reduced surface energy, which is usually called grain boundary surface phase transition. However, grain boundary engineering usually does not introduce a large number of dislocations, which is a significant limitation for chalcogenides. Summary of the invention
[0004] In view of the above, the present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a gallium-containing bismuth telluride-based thermoelectric material and a preparation method thereof. The gallium-containing bismuth telluride-based thermoelectric material provided by the present invention has the advantages of high microhardness and high structural stability. At the same time, the preparation method has a simple process flow and is suitable for application in large-scale industrial production.
[0005] To this end, in a first aspect, an embodiment of the present invention provides a gallium-containing bismuth telluride-based thermoelectric material, wherein the gallium-containing bismuth telluride-based thermoelectric material is divided into p-type and n-type, and the chemical formulas thereof are respectively Bi 2-y-x Sb y Ga x Te3 and Bi 2-x Ga x Te 3-z Se z , where the value range of x is: 0<x≤0.05, the value range of y is: 0≤y≤2, and the value range of z is: 0≤z≤3.
[0006] Preferably, the chemical formulas of the gallium-containing bismuth telluride-based thermoelectric materials are Bi 0.35-x Sb 1.65 Ga x Te3 and Bi 2- x Ga x Te 2.7 Se 0.3 , where the value range of x is: 0<x≤0.05.
[0007] In a second aspect, an embodiment of the present invention provides a method for preparing the gallium-containing bismuth telluride-based thermoelectric material provided in the first aspect, the preparation method comprising: weighing and mixing each element according to the chemical formula of the gallium-containing bismuth telluride-based thermoelectric material to obtain a mixture, and packaging it; smelting the packaged mixture at a high temperature to allow the mixture to fully react in a high-temperature molten state, and then annealing to obtain a metal ingot; placing the metal ingot in a ball mill, and after adding ball mill beads of different diameters in a certain proportion, ball milling the metal ingot to obtain a powder material; placing the powder material in a graphite mold, performing vacuum discharge plasma sintering and thermal deformation treatment, and obtaining the gallium-containing bismuth telluride-based thermoelectric material after cooling.
[0008] Preferably, the mixture is placed in a quartz tube, which is sealed with an oxyhydrogen flame to form a closed high vacuum tube environment and purged with argon gas to prevent oxidation of the mixture.
[0009] Preferably, in the mixture, the purity of each element is greater than 99.999%.
[0010] Preferably, the packaged mixture is placed in a muffle furnace, which is heated to 700-900°C at a rate of 80-150°C per hour, kept warm for 400-700 minutes, then cooled to 600-700°C within 220 minutes, kept warm for 400-700 minutes, and finally cooled to room temperature to obtain the metal ingot.
[0011] Preferably, the diameters of the ball milling beads are 15 mm, 12 mm, 7 mm, and 5 mm, respectively, and the ball milling beads with diameters from large to small are placed in the ball milling jar in a ratio of 1:3:10:22.
[0012] Preferably, the ball mill has a rotation speed of 800-1200 r / min and a ball milling time of 15-30 min.
[0013] Preferably, the graphite mold has a structure of graphite base-graphite gasket-graphite paper-powder material-graphite paper-graphite gasket-pressure rod from bottom to top.
[0014] Preferably, the spark plasma sintering process is: heating by electric current, heating to 450-550°C at a rate of 80-150°C per minute, adjusting the pressure to 50-70MPa, and sintering at a temperature of 5-20min; the thermal deformation process is: sintering in sequence by changing the mold from small to large during sintering, the diameter of the small mold is 15mm, and the diameter of the large mold is 20mm.
[0015] The gallium-containing bismuth telluride-based thermoelectric material and the preparation method thereof provided in the embodiment of the present invention are provided by 2-y Sb y Te3-based and n-type Bi2Te 3-z Se z Gallium is doped on the basis of the base thermoelectric material, in which gallium exists in the form of a nano second phase near the grain boundary and solidifies abnormally, thereby synergistically regulating the transport of carriers and phonons, as well as its introduction of point defects in the matrix and its "lubricant" effect at the grain boundary, which indirectly enhances the texture. In addition, during the solidification process, the volume of Ga expands by about 3.2%, while the volume of the solid matrix shrinks as the temperature decreases. This difference intensifies the internal stress and leads to the formation of a large number of dislocation lines and dislocation networks. With the help of the many effects of Ga in gallium-containing bismuth telluride-based thermoelectric materials, the carrier mobility μ and the lattice thermal conductivity κ are decoupled. L , thereby optimizing the thermoelectric performance, and having the advantages of high microhardness and high structural stability. At the same time, the preparation method provided by the present invention has a simple process flow, low production cost, and is suitable for application in large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 A flow chart of a method for preparing gallium-containing bismuth telluride-based thermoelectric material provided in an embodiment of the present invention;
[0017] Figure 2 A schematic diagram of an experimental process for preparing a gallium-containing bismuth telluride-based thermoelectric material provided in an embodiment of the present invention;
[0018] Figure 3 a is an XRD pattern of the p-type gallium-containing bismuth telluride-based thermoelectric material prepared in Examples 1-4 of the present invention; Figure 3 b is an XRD pattern of the n-type gallium-containing bismuth telluride-based thermoelectric material prepared in Example 5-9 of the present invention;
[0019] Figure 4 a. Figure 4 b. Figure 4 c is a low-magnification STEM-HAADF image of the gallium-containing bismuth telluride-based thermoelectric material prepared in Example 1 of the present invention;
[0020] Figure 4 d is a high-resolution HAADF image of the gallium-containing bismuth telluride-based thermoelectric material prepared in Example 1 of the present invention;
[0021] Figure 4 e. Figure 4 f is the corresponding EDS image of the gallium nano-precipitates of the gallium-containing bismuth telluride-based thermoelectric material prepared in Example 1 of the present invention;
[0022] Figure 5 a. Figure 5 b are respectively a low-magnification STEM-ABF image and a corresponding EDS image of the dislocation network region of the gallium-containing bismuth telluride-based thermoelectric material prepared in Example 1 of the present invention;
[0023] Figure 5 c is a STEM-HAADF image and FFT image of the dislocation-free region of the gallium-containing bismuth telluride-based thermoelectric material prepared in Example 1 of the present invention;
[0024] Figure 5 d is a low-magnification STEM-ABF image of the dislocation line region of the gallium-containing bismuth telluride-based thermoelectric material prepared in Example 1 of the present invention;
[0025] Figure 5 e. Figure 5 f is Figure 5 Enlarged image in d;
[0026] Figure 5 g is the IFFT image and GPA result of the gallium-containing bismuth telluride-based thermoelectric material prepared in Example 1 of the present invention;
[0027] Figure 6 for Figure 5 Schematic diagram of the formation of dislocation described in . DETAILED DESCRIPTION
[0028] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0029] The disclosure below provides many different embodiments or examples to implement different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or letters in different examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides examples of various specific processes and materials, but those of ordinary skill in the art can appreciate the reusability of other processes and / or the use of other materials.
[0030] The purpose of the present invention is to provide a gallium-containing bismuth telluride-based thermoelectric material and a preparation method thereof. The gallium-containing bismuth telluride-based thermoelectric material provided by the present invention has the advantages of high thermoelectric performance and high structural stability due to the introduction of elemental gallium decoupling carrier mobility and lattice thermal conductivity. At the same time, the preparation method provided by the present invention has a simple process flow, low production cost, and is suitable for application in large-scale industrial production.
[0031] The first embodiment of the present invention provides a gallium-containing bismuth telluride-based thermoelectric material, wherein the chemical formula of the gallium-containing bismuth telluride-based thermoelectric material is p-type Bi 2-y-x Sb y Ga x Te3 and n-type Bi 2-x Ga x Te 3-z Se z , wherein the value range of x is: 0<x≤0.05, the value range of y is: 0≤y≤2, and the value range of z is: 0≤z≤3. The gallium-containing bismuth telluride-based thermoelectric material provided by the present invention is 2-y Sb y Te3-based and n-type Bi2Te 3-z Se z Gallium is doped on the basis of the base thermoelectric material, in which gallium exists in the form of a nanosecond phase near the grain boundary. With the help of its abnormal solidification, the transport of carriers and phonons is synergistically regulated, as well as its introduction of point defects in the matrix and its "lubricant" effect near the grain boundary, which decouples the carrier mobility μ and the lattice thermal conductivity κ. L , thereby optimizing the thermoelectric performance and having the advantages of high microhardness and high structural stability.
[0032] Preferably, when x=0.02 and y=1.63, the chemical formula of the p-type gallium-containing bismuth telluride-based thermoelectric material is Bi 0.35 Sb 1.63 Ga 0.02 Te3, at this time, the p-type gallium-containing bismuth telluride-based thermoelectric material obtained a maximum zT value of 1.53 at 375K.
[0033] Preferably, when x=0.01 and z=0.3, the chemical formula of the n-type gallium-containing bismuth telluride-based thermoelectric material is Bi 1.99 Ga 0.01 Te 2.7 Se 0.3 At this time, the n-type gallium-containing bismuth telluride-based thermoelectric material obtained a maximum zT value of 1.06 at 425K.
[0034] The second embodiment of the present invention provides a method for preparing a gallium-containing bismuth telluride-based thermoelectric material, such as Figure 1 and Figure 2 As shown, the preparation method comprises the following steps:
[0035] Step S1: weighing and mixing the single substances of the elements according to the general chemical formula of the gallium-containing bismuth telluride-based thermoelectric material to obtain a mixed material, and then packaging the mixed material;
[0036] Specifically, a quartz tube with an outer diameter of 20 mm and an inner diameter of 17 mm can be selected, the grooves can be burned and cleaned, the mixture can be placed in the quartz tube, and the quartz tube can be sealed with a hydrogen-oxygen flame to form a closed high vacuum tube environment to 1×10 -3 Pa and argon gas is used for washing to prevent the mixed material from oxidation. In addition, the purity of each element is greater than 99.999%.
[0037] Step S2: melting the packaged mixed material at high temperature to allow the mixed material to fully react in a high temperature molten state, and then annealing to obtain a metal ingot;
[0038] Specifically, the packaged mixture is placed in a muffle furnace, which is heated to 700-900°C at a rate of 80-150°C per hour, and kept warm for 400-700 minutes; then the mixture is cooled to 600-700°C within 220 minutes, kept warm for 400-700 minutes, and finally cooled to room temperature to obtain the metal ingot.
[0039] Preferably, the muffle furnace is heated at a rate of 100°C per hour to 800°C and then kept at that temperature for 600 minutes, then cooled to 650°C within 220 minutes and then kept at that temperature for 600 minutes, and finally cooled to room temperature within 220 minutes, and then the metal ingot is taken out from the quartz tube.
[0040] In this step, when each element particle is smelted to form an alloy ingot, if the smelting temperature is too low (for example, the smelting temperature is lower than 700°C), the element particles will not be fully smelted, and the obtained alloy ingot may contain impurities, which will affect the performance of the thermoelectric material; if the smelting temperature is too high (for example, the smelting temperature is higher than 900°C), the quartz tube may soften, even melt, or explode during the smelting of the single particle. This embodiment controls the smelting temperature within the range of 700°C-900°C, which can not only make the single particle fully smelted, but also avoid the problem of explosion during the smelting process.
[0041] Furthermore, in the process of smelting single-element particles, the heating rate should not be too fast or too slow; the holding time should not be too long or too short; the cooling rate should not be too fast or too slow; the quenching temperature should not be too high or too low. The various ranges provided in this embodiment can not only ensure that the particles of each element are fully melted, but also avoid the generation of impurities during the smelting process.
[0042] Step S3: placing the metal ingot into a ball milling jar, and adding ball milling beads of different diameters in a certain proportion, and then ball milling the metal ingot to obtain a powder material;
[0043] The diameters of the ball milling beads are 15 mm, 12 mm, 7 mm, and 5 mm, respectively. The ball milling beads with diameters from large to small are placed in a ball milling tank in a ratio of 1:3:10:22. The ball mill speed can be 800-1200 r / min, and the ball milling time can be 15-30 min. Preferably, the ball mill speed is 1000 r / min, and the ball milling time is 20 min.
[0044] In the embodiment of the present invention, in order to prevent the metal ingot from being oxidized during the ball milling process, the ball milling jar may be vacuumed. Furthermore, after the ball milling is completed, the powder is taken out and then hand-ground using an agate mortar until it becomes a uniform and fine powder to obtain a powder material.
[0045] Step S4: placing the powder material in a graphite mold, performing vacuum discharge plasma sintering and thermal deformation treatment, and obtaining the gallium-containing bismuth telluride-based thermoelectric material after cooling.
[0046] The structure of graphite base-graphite gasket-graphite paper-powder-graphite paper-graphite gasket-pressure rod is formed from bottom to top inside the graphite mold. The spark plasma sintering process is: heating with electric current at a rate of 80-150°C per minute to 450-550°C, adjusting the pressure to 50-70MPa, and sintering at a temperature of 500°C and pressure for 5-20min. Preferably, the spark plasma sintering process is: heating at a rate of 100°C per minute to a sintering temperature of 500°C, and keeping the temperature at a sintering pressure of 50MPa for 5min.
[0047] In addition, under the same sintering process as mentioned above, the thermal deformation process is as follows: the first step is to use a mold with a diameter of 15 mm to sinter a small ingot, and the second step is to put the ingot with a diameter of 15 mm into a mold with a diameter of 20 mm and pressurize and sinter it into a 20 mm ingot to achieve thermal deformation.
[0048] The gallium-containing bismuth telluride-based thermoelectric material prepared by the above-mentioned preparation method of the gallium-containing bismuth telluride-based thermoelectric material uses the most common commercial p-type Bi 2-y Sb y Te3 and n-type Bi2Te 3-z Se z Thermoelectric materials, and the introduction of single element gallium, through its abnormal solidification near the matrix grain boundary synergistically regulates the transport of carriers and phonons. The selection of gallium has the following beneficial effects:
[0049] 1. Replacing antimony with gallium will transfer the orbital electrons of gallium to the p orbital, creating a neutral point defect, thereby minimizing the fluctuation of carrier concentration (n);
[0050] 2. Given the inherently low solid solubility of gallium in V2VI3-based alloys (less than 1%), it mainly forms gallium nanoprecipitates near grain boundaries;
[0051] 3. Gallium has a relatively low melting point of about 303K, which is much lower than the temperature used in SPS or HD processes (723K), which helps to generate a transient liquid phase at the grain boundary. During the HD process, this liquid phase acts as a "lubricant", thereby enhancing the (00l) texture;
[0052] 4. Low-energy carriers are selectively scattered when passing through the interface barrier between the gallium nanoprecipitates and the matrix, thereby increasing the effective mass of the state density (m*);
[0053] 5. During the solidification process, the volume of gallium expands by about 3.2%, while as the temperature decreases, the volume of the solid matrix shrinks. This difference exacerbates the internal stress and leads to the formation of a large number of dislocation lines and dislocation networks;
[0054] Through these advantages, the gallium-doped anomalous grain boundary solidification strategy can simultaneously enhance the thermoelectric performance of both p-type and n-type gallium-containing bismuth telluride-based thermoelectric materials.
[0055] The following examples are further listed to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0056] Example 1
[0057] This embodiment provides a method for preparing a gallium-containing bismuth telluride-based thermoelectric material. The chemical formula of the gallium-containing bismuth telluride-based thermoelectric material prepared in this embodiment is Bi 0.35 Sb 1.63 Ga 0.02 Te3 (x=0.02, y=1.63 at this time), including the following steps:
[0058] According to the chemical formula Bi 0.35 Sb 1.63 Ga 0.02 Te3, weigh the single element raw materials Bi, Sb, Ga, Te (the purity of each element is ≥99.999%) according to the stoichiometric ratio, put the prepared raw materials into a quartz tube, and seal the quartz tube with a hydrogen-oxygen flame to form a closed high vacuum tube environment to 1×10 -3 Pa, vacuum packaging is performed; the sealed quartz tube is placed in a muffle furnace and heated, and the melting furnace is heated to 800°C at a rate of 100°C per hour and kept warm for 600 minutes to allow the mixture to fully react in a high-temperature molten state, then cooled to 650°C within 220 minutes and kept warm for 600 minutes, and finally cooled to room temperature within 220 minutes, and then the metal ingot is taken out of the quartz tube. The metal ingot is placed in a ball mill, and ball mill beads with diameters of 15 mm, 12 mm, 7 mm, and 5 mm are placed in the ball mill in a ratio of 1:3:10:22. The ball mill speed is 1000 r / min, the ball milling time is 20 min, and a powder material is obtained after sufficient grinding. Subsequently, vacuum discharge plasma sintering is performed, and molds with diameters of 15 mm and 20 mm are used successively to increase the temperature to a sintering temperature of 500° C. at a rate of 100° C. per minute, the sintering pressure is maintained at 50 MPa, the insulation time is 5 min, and the gallium-containing bismuth telluride-based thermoelectric material is obtained after cooling.
[0059] Among them, the sintering of molds with diameters of 15mm and 20mm is successively used to realize the thermal deformation process. The application of this process helps to achieve the enhancement of dislocations and textures.
[0060] Example 2
[0061] The preparation process of the gallium-containing bismuth telluride-based thermoelectric material in this embodiment 2 is similar to that in embodiment 1, except that: x=0.01, y=1.64, and the chemical formula of the gallium-containing bismuth telluride-based thermoelectric material is Bi 0.35 Sb 1.64 Ga 0.01 Te3.
[0062] Example 3
[0063] The preparation process of the gallium-containing bismuth telluride-based thermoelectric material in this embodiment 3 is similar to that in embodiment 1, except that: x=0.03, y=1.62, and the chemical formula of the gallium-containing bismuth telluride-based thermoelectric material is Bi 0.35 Sb 1.62 Ga 0.03 Te3.
[0064] Example 4
[0065] The preparation process of the gallium-containing bismuth telluride-based thermoelectric material in this embodiment 4 is similar to that in embodiment 1, except that: x=0.05, y=1.60, and the chemical formula of the gallium-containing bismuth telluride-based thermoelectric material is Bi 0.35 Sb 1.60 Ga 0.05 Te3.
[0066] Example 5
[0067] The preparation process of the gallium-containing bismuth telluride-based thermoelectric material in this embodiment 5 is similar to that in embodiment 1, except that: x=0.01, z=0.3, and the chemical formula of the gallium-containing bismuth telluride-based thermoelectric material is Bi 1.99 Ga 0.01 Te 2.7 Se 0.3 .
[0068] Example 6
[0069] The preparation process of the gallium-containing bismuth telluride-based thermoelectric material in this embodiment 6 is similar to that in embodiment 1, except that: x=0.02, z=0.3, and the chemical formula of the gallium-containing bismuth telluride-based thermoelectric material is Bi 1.98 Ga 0.02 Te 2.7 Se 0.3 .
[0070] Example 7
[0071] The preparation process of the gallium-containing bismuth telluride-based thermoelectric material in this embodiment 7 is similar to that in embodiment 1, except that: x=0.03, z=0.3, and the chemical formula of the gallium-containing bismuth telluride-based thermoelectric material is Bi 1.97 Ga 0.03 Te 2.7 Se 0.3 .
[0072] Example 8
[0073] The preparation process of the gallium-containing bismuth telluride-based thermoelectric material in this embodiment 8 is similar to that in embodiment 1, except that: x=0.04, z=0.3, and the chemical formula of the gallium-containing bismuth telluride-based thermoelectric material is Bi 1.96 Ga 0.04 Te 2.7 Se 0.3 .
[0074] Example 9
[0075] The preparation process of the gallium-containing bismuth telluride-based thermoelectric material in this embodiment 9 is similar to that in embodiment 1, except that: x=0.05, z=0.3, and the chemical formula of the gallium-containing bismuth telluride-based thermoelectric material is Bi 1.95 Ga 0.05 Te 2.7 Se 0.3
[0076] The gallium-containing bismuth telluride-based thermoelectric materials prepared in the above Examples 1-9 were tested, wherein Figure 3 XRD of gallium-containing bismuth telluride-based thermoelectric materials prepared in Examples 1-9; Figure 4 and Figure 5 TEM image of the gallium-containing bismuth telluride-based thermoelectric material prepared in Example 1, wherein Figure 4 The nano-precipitated phase of gallium in the gallium-containing bismuth telluride-based thermoelectric material prepared in Example 1, Figure 5 The dislocation network formed by gallium induction of the gallium-containing bismuth telluride-based thermoelectric material prepared in Example 1; Figure 6 for Figure 5 Schematic diagram of the formation of dislocation described in .
[0077] According to the above embodiments and the comparison of the test results obtained by testing them, it can be seen that the preparation method provided by the embodiment of the present invention is effective in p-type Bi 2-y Sb y Te3 and n-type Bi2Te 3-z Se z Gallium is introduced into thermoelectric materials, and it mainly exists in the form of nanophase near the grain boundary, forming a potential barrier with the matrix material, selectively scattering low-energy carriers, and increasing the effective mass of state density. On the other hand, due to the low melting point of gallium itself and the abnormal grain boundary solidification during thermal deformation, the orientation texture is enhanced and a high-density dislocation network is formed, which increases the effective mass of state density while suppressing the lattice thermal conductivity. Finally, the highest zT value of 1.53 was obtained for p-type materials at 375K, and the highest zT value of 1.06 was obtained for n-type materials at 425K.
[0078] In summary, the gallium-containing bismuth telluride-based thermoelectric material provided in the embodiment of the present invention introduces the decoupled carrier mobility and lattice thermal conductivity of single gallium during the preparation process, and thus has the advantages of high thermoelectric performance and high structural stability. At the same time, the preparation method provided by the present invention has a simple process flow, low production cost, and is suitable for application in large-scale industrial production.
[0079] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0080] Although embodiments of the present invention have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. A gallium-containing bismuth telluride-based thermoelectric material, characterized in that: The gallium-containing bismuth telluride-based thermoelectric material is divided into p-type and n-type, and its chemical formula is Bi 2-y-x Sb y Ga x Te3 and Bi 2-x Ga x Te 3-z Se z , where the value range of x is: 0<x≤0.05, the value range of y is: 0≤y≤2, and the value range of z is: 0≤z≤3.
2. The gallium-containing bismuth telluride-based thermoelectric material according to claim 1, characterized in that: The chemical formulas of the gallium-containing bismuth telluride-based thermoelectric materials are respectively Bi 0.35-x Sb 1.65 Ga x Te3 and Bi 2-x Ga x Te 2.7 Se 0.3 , where the value range of x is: 0<x≤0.
05.
3. A method for preparing the gallium-containing bismuth telluride-based thermoelectric material according to claim 1, characterized in that: The preparation method comprises: According to the general chemical formula of the gallium-containing bismuth telluride-based thermoelectric material, each element is weighed and mixed to obtain a mixed material, and then packaged; The encapsulated mixed material is melted at high temperature to make the mixed material fully react in a high temperature molten state, and then annealed to obtain a metal ingot; The metal ingot is placed in a ball mill, and after ball milling beads of different diameters are added in a certain proportion, the metal ingot is ball milled to obtain a powder material; The powder material is placed in a graphite mold, subjected to vacuum discharge plasma sintering and thermal deformation treatment, and the gallium-containing bismuth telluride-based thermoelectric material is obtained after cooling.
4. The method for preparing gallium-containing bismuth telluride-based thermoelectric material according to claim 3, characterized in that: The mixed material is placed in a quartz tube, which is sealed with an oxyhydrogen flame to form a closed high vacuum tube environment, and argon gas is used for purging to prevent the mixed material from being oxidized.
5. The method for preparing gallium-containing bismuth telluride-based thermoelectric material according to claim 3, characterized in that: In the mixed material, the purity of each element is greater than 99.999%.
6. The method for preparing gallium-containing bismuth telluride-based thermoelectric material according to claim 3, characterized in that: The packaged mixture is placed in a muffle furnace, which is heated to 700-900°C at a rate of 80-150°C per hour, kept warm for 400-700 minutes, then cooled to 600-700°C within 220 minutes, kept warm for 400-700 minutes, and finally cooled to room temperature to obtain the metal ingot.
7. The method for preparing gallium-containing bismuth telluride-based thermoelectric material according to claim 3, characterized in that: The diameters of the ball milling beads are 15 mm, 12 mm, 7 mm, and 5 mm, respectively. The ball milling beads with diameters from large to small are placed in the ball milling jar in a ratio of 1:3:10:
22.
8. The method for preparing gallium-containing bismuth telluride-based thermoelectric material according to claim 3, characterized in that: The ball mill has a rotation speed of 800-1200 r / min and a ball milling time of 15-30 min.
9. The method for preparing gallium-containing bismuth telluride-based thermoelectric material according to claim 3, characterized in that: The graphite mold has a structure of graphite base-graphite gasket-graphite paper-powder material-graphite paper-graphite gasket-pressing rod from bottom to top.
10. The method for preparing gallium-containing bismuth telluride-based thermoelectric material according to claim 3, characterized in that: The spark plasma sintering process is: using electric current to heat, heating at a rate of 80-150°C per minute to 450-550°C, adjusting the pressure to 50-70MPa, and sintering at a temperature of 5-20min; the thermal deformation process is: sintering in sequence by changing the mold from small to large during sintering, the small mold has a diameter of 15mm, and the large mold has a diameter of 20mm.