Modified molecular sieve loaded with silver-containing ionic liquid as well as preparation method and application of modified molecular sieve
Through the modified molecular sieve loaded with silver-containing ionic liquid, the problems of poor selectivity and high cost in the separation process of ethylene and ethane are solved, and efficient and low-cost ethylene separation effect is achieved, and good cycle stability and adsorption speed are achieved.
Patent Information
- Application Number
- CN202411165086.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art has problems such as poor selectivity, high cost and high equipment requirements in the separation process between ethylene and ethane, and the existing separation methods have low recovery rates for ethylene.
Modified molecular sieve loaded with silver ion liquid is formed by reacting imidazole ionic liquid with nanosilic salt under ultrasonic conditions, combined with organic silane-modified molecular sieve to form a modified molecular sieve loaded with silver ionic liquid for selectivity Adsorption and separation of ethylene gas.
High selective adsorption and efficient separation of ethylene are achieved, and the preparation method is simple, low cost, good cycle stability and fast adsorption speed.
Smart Images

Figure BDA0005007621600000131 
Figure BDA0005007621600000151
Abstract
Description
Technical Field
[0001] The invention relates to the fields of gas separation and purification and ionic liquid application, and in particular to a modified molecular sieve loaded with silver-containing ionic liquid and a preparation method and application thereof. Background Art
[0002] This section provides background information related to the present application which does not necessarily constitute prior art.
[0003] As an important source of energy and chemicals, the petrochemical industry has made improving its production efficiency and product quality an important direction of industry development. As an extremely important basic raw material in the petrochemical industry, the optimization of ethylene separation technology is of great significance to improving production efficiency and reducing production costs. Ethylene (C2H4) and ethane (C2H6) are one of the main gas products produced during the cracking of petroleum. As an important chemical raw material, ethylene is widely used in the production of polyethylene, ethylene oxide, ethanol and other chemical products. However, due to the very similar physical and chemical properties of ethylene and ethane, the separation of ethylene and ethane has become a technical problem.
[0004] At present, the separation methods of ethylene and ethane in industry include cryogenic distillation, intercooling oil absorption, membrane separation and pressure swing adsorption separation. Among them, cryogenic distillation has high requirements for equipment, and this method needs to be at a higher pressure and extremely low temperature to achieve efficient separation of ethylene and ethane, so it has high energy consumption; the intercooling oil absorption method mainly uses C3-C5 mixed aromatics as absorbents to achieve separation by utilizing the different solubility of ethylene and ethane in the absorbent, but C3-C5 mixed aromatics have a low boiling point and large loss; the membrane separation method is mainly based on the different permeation rates of ethylene and ethane in the membrane to form a certain partial pressure difference on both sides of the membrane. This method has high requirements for membrane materials, a short membrane service life and a low processing capacity; the pressure swing adsorption method requires a multi-stage adsorption device to achieve a continuous and efficient separation effect.
[0005] CN109651055A discloses a method for separating ethylene and ethane, the method comprising: contacting a mixed gas of ethylene and ethane with an ultra-microporous anion pillared hybrid material, the ultra-microporous anion pillared hybrid material selectively adsorbing ethylene molecules, and separating ethylene from ethane; the absorption amount of ethylene by the separation method is 1.5-2.5 mmol / g, but the selectivity is poor. CN109748770A discloses an ethylene and ethane adsorption separation method based on an ultra-microporous metal organic framework material, the method comprising: contacting a mixed gas of ethylene and ethane with an ultra-microporous metal organic framework material, adsorbing ethylene in the mixed gas, and separating ethylene from ethane; the separation method can achieve selective adsorption of ethylene, but the ultra-microporous metal organic framework material has a high cost and a low ethylene recovery rate. CN104277880A discloses a method for absorbing and separating light hydrocarbons from dry gas or industrial tail gas by using ionic liquid. The steps of absorbing and separating light hydrocarbons are as follows: using ionic liquid as absorbent, contacting with dry gas or industrial tail gas, absorbing to obtain an absorption liquid containing light hydrocarbons, and then desorbing and separating to obtain light hydrocarbons; the light hydrocarbons are mainly alkanes or olefins containing C2 to C4; the ionic liquid is tetrabutylphosphonium octanoate, but the separation selectivity of the method for olefins is not high. CN107398146A discloses a protonated ionic liquid absorbent containing a metal salt and its application. The absorbent includes a protonated ionic liquid as a solvent and a metal silver salt as an olefin complexing carrier, but Ag + It is unstable in ionic liquids and is easily deactivated and reduced to nanosilver. CN108187607A discloses an adsorption separation agent for separating ethylene and ethane and a preparation method thereof, the separation method comprising: contacting a mixed gas of ethylene and ethane with an adsorption separation agent composed of a titanium silicon molecular sieve carrier and a metal salt active component, the adsorption separation machine selectively adsorbs ethylene molecules to separate ethylene and ethane; the separation factor of the adsorbent for ethylene and ethane is only 6.57 at most, and the selectivity is poor. CN105251442A discloses an adsorbent for efficiently separating ethylene and ethane, the separation method comprising: contacting a mixed gas of ethylene and ethane with an adsorption material loaded with cuprous chloride, selectively adsorbing ethylene gas, and separating ethylene and ethane; the separation method can achieve selective adsorption of ethylene, but the selectivity of ethylene and ethane is only 8.25 at most, and the selectivity is poor.
[0006] Therefore, in order to solve the above problems, it is necessary to develop an adsorption separation agent for ethylene and ethane separation with low cost and high selectivity, so as to achieve high absorption and selectivity of olefins. Through the research on absorption separation of olefins / alkanes, the following knowledge is obtained:
[0007] 1. In order to improve the selectivity of olefin / alkane separation, metal complex absorption is used for olefin / alkane separation. +It has the ability to complex with double bonds in olefins, and the resulting coordination compounds are easy to desorb, and can be cyclically absorbed and desorbed to separate low-carbon olefins and alkanes;
[0008] 2. Molecular sieves, as a new type of separation material, have a regular pore structure and a high specific surface area, and can selectively separate different components in a mixed gas through molecular sieving and adsorption. However, it is often difficult to achieve the ideal separation effect by relying solely on the adsorption capacity of molecular sieves. Ionic liquids, as a new type of green solvent, show great potential in the field of gas separation due to their low volatility, high thermal stability and good solubility, but their high viscosity affects their fluidity and mass transfer performance. Molecular sieves are combined with ionic liquids to form a new type of composite material, which can utilize the pore structure of molecular sieves and the excellent adsorption properties of ionic liquids to achieve efficient separation of ethylene and ethane. However, there are no reports on the combination of molecular sieves and ionic liquids for the separation of ethylene and ethane. Summary of the invention
[0009] The object of the present invention is to provide a modified molecular sieve loaded with silver ion liquid, which can be used as an adsorption separation agent for selective adsorption separation and recovery of ethylene gas in ethylene-ethane mixed gas, thereby achieving separation and purification of ethylene gas in ethylene-ethane mixed gas.
[0010] To achieve the above object, the present invention adopts the following technical scheme: a modified molecular sieve loaded with silver ion liquid, comprising a modified molecular sieve and a silver ion liquid loaded on the modified molecular sieve, wherein:
[0011] The modified molecular sieve is one or more of SAPO-34, MCM-41, MCM-48, SBA-15, SBA-16, KIT-6, FDU-12, HMS, TUD-1 modified with organosilane;
[0012] The silver-containing ionic liquid is a functionalized imidazole ionic liquid containing silver salt. For the modified molecular sieve, the loading amount of the silver-containing ionic liquid is 10% to 450%. If the loading amount is lower than 10%, the adsorption effect of the modified molecular sieve loaded with the silver-containing ionic liquid is poor; if the loading amount is higher than 450%, the silver-containing ionic liquid cannot be completely loaded onto the modified molecular sieve, resulting in a semi-solid state.
[0013] The preparation method of the modified molecular sieve loaded with silver ion liquid provided by the present invention comprises the following steps:
[0014] The process of reacting an imidazole ionic liquid with a nano-sized silver salt under ultrasonic conditions to obtain a silver ion liquid;
[0015] A step of mixing the organosilane and the first organic solvent, adding the molecular sieve, and stirring the mixture in an environment without water or oxygen to obtain a first mixture;
[0016] A step of washing the first mixture solvent with a first organic solvent and then vacuum drying to remove the first organic solvent to obtain a modified molecular sieve;
[0017] A step of uniformly mixing the silver ion liquid, the surfactant and the second organic solvent under ultrasonic conditions and then adding the modified molecular sieve to obtain a second mixture;
[0018] The second mixture is placed in a rotary evaporator for rotary heating, and then the second organic solvent is removed by vacuuming in the rotary evaporator to obtain a modified molecular sieve loaded with a silver ion liquid.
[0019] In one or more embodiments, the cation of the imidazole ionic liquid is one or more of 1,3-dimethylimidazolium, 1,3-diethylimidazolium, 1-propyl-3-methylimidazolium, 1-butyl-3-methylimidazolium, 1-hexyl-3-methylimidazolium, 1-ethyl-3-methylimidazolium, 1-octyl-3-methylimidazolium modified with carboxyl, hydroxyl or amino groups. The anion of the imidazole ionic liquid is one or more of nitrate ion, tetrafluoroborate ion and hexafluorophosphate ion.
[0020] In one or more embodiments, the nano-processed silver salt is one or more of AgNO3, AgPF6, AgBF4, AgOTf or Ag3PO4.
[0021] In one or more embodiments, the reaction time of the imidazole ionic liquid and the nano-treated silver salt under ultrasonic conditions is 1 to 36 hours, and the ultrasonic conditions meet the following conditions: the ultrasonic frequency is 20 to 60 kHz, and the power is 50 to 500W.
[0022] In one or more embodiments, the molecular sieve is one or more of SAPO-34, MCM-41, MCM-48, SBA-15, SBA-16, KIT-6, FDU-12, HMS, and TUD-1.
[0023] In one or more embodiments, the first organic solvent is one or more of anhydrous ethanol, toluene, and n-hexane; the organosilane is one or more of methyltrimethoxysilane and propyltriethoxysilane. Preferably, based on the total mass of the organosilane and the first organic solvent, the mass fraction of the organosilane is 0.1% to 40%. If the mass fraction of the organosilane is lower than 0.1%, the molecular sieve cannot be fully modified, the functional groups formed on the surface are reduced, and the loading amount and loading speed of the ionic liquid are reduced; if the mass fraction of the organosilane is higher than 40%, the organosilane will be deposited in the pores of the molecular sieve, blocking the pores, reducing the specific surface area and pore volume of the molecular sieve, and affecting the adsorption performance.
[0024] In one or more embodiments, the organosilane and the first organic solvent are mixed, and then molecular sieves are added and stirred for reaction in an environment without water or oxygen. The stirring reaction time is 1 to 12 hours.
[0025] In one or more embodiments, the first mixture solvent is vacuum dried to meet the following conditions: drying temperature is 100-200° C., vacuum pressure is 1-50 kPa, and time is 1-24 hours.
[0026] In one or more embodiments, the surfactant is one or more of sodium dodecyl sulfate (SDS), polyoxyethylene nonylphenol ether (NP-10), polyethylene glycol octylphenyl ether (Triton X-100), and polypropylene glycol polyethylene glycol block copolymer (Pluronic F-127); the second organic solvent is one or more of anhydrous ethanol, dichloroethane, acetonitrile, dichloromethane, methanol, ethylene glycol dimethyl ether, and ethyl acetate. For the mass ratio of the second organic solvent to the silver-containing ion liquid, if it is too low, the silver-containing ion liquid will not be completely dissolved, thereby affecting the loading effect; if it is too high, it will lead to a long evaporation time and waste of organic solvent. For the mass ratio of the second organic solvent to the surfactant, if it is too low, the interfacial tension between the silver-containing ion liquid and the molecular sieve cannot be effectively reduced, resulting in a reduction in the loading amount and uniformity of the silver-containing ion liquid; if it is too high, a surfactant layer will be formed on the surface of the molecular sieve or the pores will be blocked, affecting the adsorption effect. Preferably, the mass ratio of the second organic solvent to the silver ion liquid is 1:1 to 100:1, and the mass ratio of the second organic solvent to the surfactant is 19:1 to 999:1.
[0027] In one or more embodiments, the silver ion liquid, the surfactant and the second organic solvent are mixed under ultrasonic conditions for 10 to 60 minutes, and the ultrasonic conditions meet the following conditions: the ultrasonic frequency is 20 to 60 kHz and the power is 50 to 500 W.
[0028] In one or more embodiments, the rotary heating satisfies: the temperature is 40 to 140° C. and the time is 4 to 24 hours.
[0029] The invention also provides application of the modified molecular sieve loaded with silver ion liquid in separation of olefins / alkanes.
[0030] In one or more embodiments, the modified molecular sieve loaded with silver ion liquid provided by the present invention is loaded into an adsorption column as an adsorption separation agent, and then a mixed gas containing ethylene and ethane is introduced into the adsorption column. At a certain temperature and pressure, the modified molecular sieve loaded with silver ion liquid provided by the present invention will selectively adsorb ethylene gas. After the adsorption, the modified molecular sieve can desorb ethylene gas at a certain temperature and pressure, thereby achieving the separation and purification of ethylene gas.
[0031] Preferably, when the modified molecular sieve loaded with silver ion liquid provided by the present invention adsorbs ethylene gas: the adsorption temperature is 20 to 70° C., and the adsorption pressure is 0.1 to 3.0 MPa;
[0032] Preferably, when the modified molecular sieve loaded with silver ion liquid provided by the present invention desorbs ethylene gas: the desorption temperature is 100-200°C, and the desorption pressure is 1×10 -5 Pa~50kPa.
[0033] Compared with the prior art, the present invention has the following effective effects:
[0034] The modified molecular sieve loaded with silver ion liquid provided by the invention has high selectivity for olefins, good cycle stability and fast adsorption speed.
[0035] The preparation method of the modified molecular sieve loaded with silver ion liquid provided by the invention is simple and easy to operate, has low cost, low equipment investment, and the solvent can be recycled and has no by-products.
[0036] The following describes the invention in conjunction with specific embodiments. DETAILED DESCRIPTION
[0037] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.
[0038] Example 1
[0039] This embodiment provides a modified molecular sieve loaded with a silver ion liquid, and the preparation method thereof comprises the following steps:
[0040] (1) SAPO-34 molecular sieve was selected, and propyltriethoxysilane was used to carry out surface modification reaction in anhydrous ethanol. The concentration of the organosilane was 15 wt %. The molecular sieve was added, and the reaction was stirred in anhydrous and oxygen-free environment. After the reaction for 6 hours, the molecular sieve was washed with anhydrous ethanol, and the modified molecular sieve was obtained after drying at 150° C. under vacuum at 20 kPa.
[0041] (2) 1-ethyl-3-carboxyethyl imidazole tetrafluoroborate and AgBF4 were reacted in a molar ratio of 2:1 under ultrasonic stirring at 20 kHz and 200 W for 24 hours to obtain a silver ion liquid.
[0042] (3) Take 20g of anhydrous ethanol and add 0.5% of the surfactant sodium dodecyl sulfate (SDS) to prepare a solvent, add 1g of the silver ion liquid dropwise to the solvent under ultrasonic stirring, and continue stirring for 30 minutes to fully dissolve; add 2g of the modified molecular sieve, heat and rotate in a rotary evaporator at 78°C for 12 hours; slowly evacuate until the solvent is completely volatilized to obtain the modified molecular sieve loaded with the silver ion liquid, wherein the loading amount of the silver ion liquid is 50% for the modified molecular sieve.
[0043] Example 2
[0044] This embodiment provides a modified molecular sieve loaded with a silver ion liquid, and the preparation method thereof comprises the following steps:
[0045] (1) MCM-41 molecular sieve was selected, and methyltrimethoxysilane was used to carry out surface modification reaction in toluene. The concentration of the organosilane was 20 wt %. The molecular sieve was added, and the reaction was stirred in an anhydrous and oxygen-free environment. After the reaction for 12 hours, the molecular sieve was washed with toluene, and the modified molecular sieve was obtained after drying at a vacuum temperature of 100° C. at 10 kPa.
[0046] (2) 1-carboxymethyl-3-methylimidazolium tetrafluoroborate and AgBF4 were reacted in a molar ratio of 1:1 under ultrasonic stirring at 40 kHz and 400 W for 36 hours to obtain a silver ion liquid.
[0047] (3) Take 100g of dichloromethane and add 1% of the surfactant polyethylene glycol octylphenyl ether (Triton X-100) to prepare a solvent, add 1g of silver ion liquid dropwise to the solvent under ultrasonic stirring, and continue stirring for 60 minutes to fully dissolve; add 2g of modified molecular sieve, heat and rotate in a rotary evaporator at 40°C for 12 hours; evacuate until the solvent is completely volatilized to obtain a modified molecular sieve loaded with silver ion liquid, wherein the loading amount of the silver ion liquid is 50% for the modified molecular sieve.
[0048] Example 3
[0049] This embodiment provides a modified molecular sieve loaded with a silver ion liquid, and the preparation method thereof comprises the following steps:
[0050] (1) Select SBA-15 molecular sieve, use methyltrimethoxysilane to carry out surface modification reaction in anhydrous ethanol, the concentration of organic silane is 10wt%, add molecular sieve, stir and react in anhydrous and oxygen-free environment, after reacting for 6 hours, use anhydrous ethanol to wash, and dry at 200°C under vacuum 5kPa to obtain modified molecular sieve.
[0051] (2) 1-aminoethyl-3-methylimidazolium hexafluorophosphate and AgPF6 were reacted at a molar ratio of 3:1 under ultrasonic stirring at 60 kHz and 100 W for 24 hours to obtain a silver ion liquid.
[0052] (3) Take 100g of ethylene dichloride and add 1% of the surfactant polyoxyethylene nonylphenol ether (NP-10) to prepare a solvent, add 1g of silver ion liquid dropwise to the solvent under ultrasonic stirring, and continue stirring for 60 minutes to fully dissolve; add 2g of modified molecular sieve, heat and rotate in a rotary evaporator at 85°C for 12 hours; evacuate until the solvent is completely volatilized to obtain a modified molecular sieve loaded with silver ion liquid, wherein the loading amount of the silver ion liquid is 50% for the modified molecular sieve.
[0053] Example 4
[0054] This embodiment provides a modified molecular sieve loaded with a silver ion liquid, and the preparation method thereof comprises the following steps:
[0055] (1) FDU-12 molecular sieve was selected, and propyltriethoxysilane was used to carry out surface modification reaction in toluene. The concentration of the organosilane was 30 wt %. The molecular sieve was added, and the reaction was stirred in an anhydrous and oxygen-free environment. After the reaction for 6 hours, the molecular sieve was washed with toluene, and the modified molecular sieve was obtained after drying at 35 kPa and 120° C. in vacuum.
[0056] (2) 1-Hydroxyethyl-3-methylimidazolium tetrafluoroborate and AgBF4 were reacted in a molar ratio of 2:1 under ultrasonic stirring at 40 kHz and 500 W for 36 hours to obtain a silver ion liquid.
[0057] (3) 100 g of ethylene dichloride and 100 g of methanol are added with 1% of a surfactant, sodium dodecyl sulfate (SDS), to prepare a solvent; 2 g of a silver ion liquid is added dropwise to the solvent under ultrasonic stirring; stirring is continued for 60 minutes to fully dissolve; 2 g of a modified molecular sieve is added; the mixture is heated at 85° C. and rotated in a rotary evaporator for 12 hours; vacuuming is performed until the solvent is completely volatilized to obtain a modified molecular sieve loaded with a silver ion liquid; and the loading amount of the silver ion liquid is 50% for the modified molecular sieve.
[0058] Example 5
[0059] This embodiment provides a modified molecular sieve loaded with a silver ion liquid, and the preparation method thereof comprises the following steps:
[0060] (1) HMS molecular sieve was selected, and propyltriethoxysilane was used to carry out surface modification reaction in anhydrous ethanol. The concentration of the organosilane was 15 wt %. The molecular sieve was added, and the reaction was stirred in anhydrous and oxygen-free environment. After reacting for 24 hours, the molecular sieve was washed with anhydrous ethanol, and dried at 45 kPa and 200° C. in vacuum to obtain the modified molecular sieve.
[0061] (2) 1-aminopropyl-3-methylimidazole nitrate and AgNO3 were reacted in a molar ratio of 1:1 under ultrasonic stirring at 50 kHz and 250 W for 24 hours to obtain a silver ion liquid.
[0062] (3) Take 200g of acetonitrile and add 1% of the surfactant sodium dodecyl sulfate (SDS) to prepare a solvent, add 2g of silver ion liquid dropwise to the solvent under ultrasonic stirring, and continue stirring for 60 minutes to fully dissolve; add 4g of modified molecular sieve, heat and rotate in a rotary evaporator at 85°C for 12 hours; evacuate until the solvent is completely volatilized to obtain a modified molecular sieve loaded with silver ion liquid, wherein the loading amount of the silver ion liquid is 50% for the modified molecular sieve.
[0063] Example 6
[0064] This embodiment provides a method for preparing a modified molecular sieve loaded with silver ion liquid. Except that the amount of ionic liquid added in step (3) is replaced by "2 g" and the loading amount of the silver ion liquid is 100%, other conditions are the same as those in Example 1.
[0065] Example 7
[0066] This embodiment provides a method for preparing a modified molecular sieve loaded with silver ion liquid. Except that the molar ratio in step (2) is 5:1, the amount of ionic liquid added in step (3) is replaced by "6 g" and the loading amount of the silver ion liquid is 300%, other conditions are the same as those in Example 1.
[0067] Example 8
[0068] The present embodiment provides a method for preparing a modified molecular sieve loaded with silver ion liquid, except that the "1-ethyl-3-carboxyethyl imidazole tetrafluoroborate" in step (2) is replaced by "1-carboxymethyl-3-methylimidazolium tetrafluoroborate" and "AgBF4" is replaced by "AgOTf", the other conditions are the same as those in Example 1.
[0069] Example 9
[0070] The present embodiment provides a method for preparing a modified molecular sieve loaded with a silver ion liquid, wherein the conditions are the same as those in Example 2 except that the "1-carboxymethyl-3-methylimidazolium tetrafluoroborate" in step (2) is replaced by "1-hydroxyethyl-3-methylimidazolium tetrafluoroborate" and the "dichloromethane" in step (3) is replaced by "anhydrous ethanol", and the rotary evaporation temperature is set to 85°C.
[0071] Example 10
[0072] This embodiment provides a method for preparing a modified molecular sieve loaded with silver ion liquid. Except that the molar ratio in step (2) is 10:1, other conditions are the same as those in Example 2.
[0073] Embodiment 11
[0074] The present embodiment provides a method for preparing a modified molecular sieve loaded with silver ion liquid, except that the "1-aminoethyl-3-methylimidazolium hexafluorophosphate" in step (2) is replaced by "1-ethyl-3-carboxyethylimidazolium tetrafluoroborate", "AgPF6" is replaced by "Ag3PO4" and the molar ratio is 1:2, the other conditions are the same as those in Example 3.
[0075] Example 12
[0076] This embodiment provides a method for preparing a modified molecular sieve loaded with silver ion liquid. Except that the "1-hydroxyethyl-3-methylimidazolium tetrafluoroborate and AgBF4" in step (2) is replaced by "1-aminopropyl-3-methylimidazolium nitrate and AgNO3", other conditions are the same as those in Example 4.
[0077] Example 13
[0078] The present embodiment provides a method for preparing a modified molecular sieve loaded with silver ion liquid, except that the "2 g" in step (3) is replaced by "8 g", the loading amount of the silver ion liquid is 200%, "acetonitrile" is replaced by "dichloromethane", and the rotary evaporation temperature is set to 40°C, the other conditions are the same as those in Example 5.
[0079] Comparative Example 1
[0080] This comparative example provides a method for preparing a modified molecular sieve. Except that step (2) is not performed, and step (3) of "adding 1 g of the ionic liquid after the reaction is completed dropwise" is not performed, and the loading amount of the silver-containing ionic liquid is adjusted to 0%, other conditions are the same as those in Example 1.
[0081] Comparative Example 2
[0082] This comparative example provides a method for preparing a modified molecular sieve. Except that step (2) is not performed, and step (3) of "adding 1 g of the ionic liquid after the reaction is completed dropwise" is not performed, and the loading amount of the silver-containing ionic liquid is adjusted to 0%, other conditions are the same as those in Example 2.
[0083] Comparative Example 3
[0084] This comparative example provides a method for preparing a modified molecular sieve. Except that step (2) is not performed, and step (3) of "adding 1 g of the ionic liquid after the reaction is completed dropwise" is not performed, and the loading amount of the silver-containing ionic liquid is adjusted to 0%, other conditions are the same as those in Example 3.
[0085] Comparative Example 4
[0086] This comparative example provides a method for preparing a modified molecular sieve. Except that step (2) is not performed, and step (3) of "adding 2 g of ionic liquid after the reaction is completed dropwise" is not performed, and the loading amount of the silver-containing ionic liquid is adjusted to 0%, other conditions are the same as those in Example 4.
[0087] Comparative Example 5
[0088] This comparative example provides a method for preparing a modified molecular sieve. Except that step (2) is not performed, and step (3) of "adding 2 g of ionic liquid after the reaction is completed dropwise" is not performed, and the loading amount of the silver-containing ionic liquid is adjusted to 0%, other conditions are the same as those in Example 5.
[0089] The modified molecular sieve loaded with silver ion liquid provided in the above-mentioned examples 1-13 and the modified molecular sieve provided in comparative examples 1-5 are respectively used as adsorption separation agents for the separation of ethylene and ethane, and the application includes: adding an adsorption separation agent to a multilayer adsorption column, the adsorption column is connected to a mixed gas adsorption device, and a mixed gas of helium, ethylene and ethane with a volume ratio of 1:2:2 is introduced, wherein helium is an internal standard gas, and adsorption is performed at 25°C and 1MPa, and the flow rate is calculated using the internal standard gas, and the tail gas is analyzed online by gas chromatography. After the outlet gas composition is stable, the actual mixed gas composition and the amount of adsorbed gas are calculated, and the results are shown in Table 1.
[0090] Table 1
[0091]
[0092] According to the results in Table 1, it can be shown that:
[0093] 1. The modified molecular sieve loaded with silver ion liquid prepared by the preparation method provided in Examples 1-13 of the present invention can achieve high absorption and high selectivity for ethylene;
[0094] 2. From the comparison between Example 1 and Examples 6-7, it can be seen that when the loading amount of the silver ion liquid is increased, the adsorption amount and selectivity of ethylene by the prepared modified molecular sieve loaded with the silver ion liquid will increase;
[0095] 3. By comparing Examples 1-5 and Comparative Examples 1-5, it can be seen that when the modified molecular sieve is not loaded with silver ion liquid, the absorption amount of ethylene is reduced and the selectivity is reduced.
[0096] The modified molecular sieve loaded with silver ion liquid prepared in Example 1 and Example 2 is applied to the separation of olefins / alkanes, and the application includes: adding 3.0g of modified molecular sieve loaded with silver ion liquid to two absorption bottles respectively, and then passing pure C2H4 gas, controlling the gas flow rate to 50mL / min, reacting at 25°C and 0.1MPa, and weighing the absorption bottle at intervals of 120min. After absorbing for 120min, ethylene is obtained by desorption separation, and the desorption conditions are: passing N2 at a flow rate of 40mL / min, desorbing at 150°C and 10kPa for 120min, and performing absorption-desorption cycles for the above operation 5 times. The absorption performance results of the modified molecular sieve loaded with silver ion liquid for ethylene are shown in Table 2.
[0097] It can be seen from Table 2 that the modified molecular sieve loaded with silver ion liquid provided by the present invention has good regeneration stability and can still maintain a high ethylene absorption capacity after multiple cycles.
[0098] Table 2
[0099]
[0100] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0101] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A modified molecular sieve loaded with a silver-containing ionic liquid, comprising a modified molecular sieve and a silver-containing ionic liquid loaded on the modified molecular sieve, characterized in that: The modified molecular sieve is one or more of SAPO-34, MCM-41, MCM-48, SBA-15, SBA-16, KIT-6, FDU-12, HMS, TUD-1 modified with organosilane; The silver-containing ionic liquid is an imidazole ionic liquid containing a silver salt; For the modified molecular sieve, the loading amount of the silver ion liquid is 10% to 450%.
2. A method for preparing a modified molecular sieve loaded with a silver ion liquid according to claim 1, characterized in that: Including the following processes: The process of reacting an imidazole ionic liquid with a nano-sized silver salt under ultrasonic conditions to obtain a silver ion liquid; A step of mixing the organosilane and the first organic solvent, adding the molecular sieve, and stirring the mixture in an environment without water or oxygen to obtain a first mixture; A step of washing the first mixture solvent with a first organic solvent and then vacuum drying to remove the first organic solvent to obtain a modified molecular sieve; A step of uniformly mixing the silver ion liquid, the surfactant and the second organic solvent under ultrasonic conditions and then adding the modified molecular sieve to obtain a second mixture; The second mixture is placed in a rotary evaporator for rotary heating, and then the second organic solvent is removed by vacuuming in the rotary evaporator to obtain a modified molecular sieve loaded with a silver ion liquid.
3. The method according to claim 2, characterized in that The cation of the imidazolium ionic liquid is one or more of 1,3-dimethylimidazolium, 1,3-diethylimidazolium, 1-propyl-3-methylimidazolium, 1-butyl-3-methylimidazolium, 1-hexyl-3-methylimidazolium, 1-ethyl-3-methylimidazolium, and 1-octyl-3-methylimidazolium modified with carboxyl, hydroxyl or amino groups; The anion of the imidazole ionic liquid is one or more of nitrate ion, tetrafluoroborate ion and hexafluorophosphate ion; The nano-processed silver salt is one or more of AgNO3, AgPF6, AgBF4, AgOTf or Ag3PO4.
4. The method according to claim 3, characterized in that The reaction time of the imidazole ionic liquid and the nano-treated silver salt under ultrasonic conditions is 1 to 36 hours, and the ultrasonic conditions meet the following conditions: the ultrasonic frequency is 20 to 60 kHz and the power is 50 to 500W.
5. The method according to claim 2, characterized in that: The molecular sieve is one or more of SAPO-34, MCM-41, MCM-48, SBA-15, SBA-16, KIT-6, FDU-12, HMS, and TUD-1; The first organic solvent is one or more of anhydrous ethanol, toluene, and n-hexane; The organosilane is one or more of methyltrimethoxysilane and propyltriethoxysilane; based on the total mass of the organosilane and the first organic solvent, the mass fraction of the organosilane is 0.1% to 40%.
6. The method according to claim 5, characterized in that After the organosilane and the first organic solvent are mixed, a molecular sieve is added and stirred for reaction in an anhydrous and oxygen-free environment for 1 to 12 hours; The first mixture solvent is vacuum dried to meet the following conditions: the drying temperature is 100-200° C., the vacuum pressure is 1-50 kPa, and the time is 1-24 hours.
7. The method according to claim 2, characterized in that The surfactant is one or more of sodium dodecyl sulfate, polyoxyethylene nonylphenol ether, polyethylene glycol octylphenyl ether, and polypropylene glycol polyethylene glycol block copolymer; The second organic solvent is one or more of anhydrous ethanol, dichloroethane, acetonitrile, dichloromethane, methanol, ethylene glycol dimethyl ether, and ethyl acetate; The mass ratio of the second organic solvent to the silver ion liquid is 1:1 to 100:1, and the mass ratio of the second organic solvent to the surfactant is 19:1 to 999:
1.
8. The method according to claim 7, characterized in that The silver ion liquid, the surfactant and the second organic solvent are mixed under ultrasonic conditions for 10 to 60 minutes, wherein the ultrasonic conditions meet the following conditions: the ultrasonic frequency is 20 to 60 kHz and the power is 50 to 500 W.
9. The method according to claim 2, characterized in that: The rotary heating meets the following requirements: the temperature is 40 to 140° C. and the time is 4 to 24 hours.
10. Use of the modified molecular sieve loaded with silver ion liquid according to claim 1 in separation of olefins / alkanes.
Citation Information
Patent Citations
Adsorption and separation agent for separation of ethylene and ethane as well as preparation method and application thereof
CN108187607A
Ionic liquid-loaded mesoporous molecular sieve as well as preparation method and application thereof
CN112076726A
Method for concentrating ethylene, separation adsorbent and preparation of separation adsorbent
CN117326912A
Silver-containing ionic liquid as well as preparation method and application thereof