Preparation method of supported transition metal catalyst, supported transition metal catalyst and application of supported transition metal catalyst in reaction for synthesizing high-carbon ketone by condensation coupling of alpha-H-containing ketone and alcohol

CN119016052APending Publication Date: 2024-11-26ZHEJIANG SAINON CHEM

Patent Information

Application Number
CN202411125706.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-24
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the synthesis method of ketones is complicated, with many by-products, high catalyst costs, harsh reaction conditions, and requires high-pressure hydrogen, low product selectivity, and difficult catalyst recovery.

Method used

Using the preparation method of a supported transition metal catalyst, a catalyst for the condensation coupling reaction between ketone and alcohol is prepared by calcining and reducing the transition metal salt and porous catalyst support under specific conditions. The catalysts include Ni5-Fe1/AC and Ni5 -Co1/AC, etc., the reaction conditions are at normal pressure, 120-250°C, and no need for solvent or high-pressure hydrogen.

Benefits of technology

A highly selective catalyzed condensation coupling reaction between ketones and small molecule alcohols can be achieved. The conversion rate of alcohols and ketones can be up to 80%, and the selectivity of target high-carbon ketones can be up to 90%, reducing the catalyst cost and simplifying the reaction process. , suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to a preparation method of a supported transition metal catalyst, the supported transition metal catalyst and application of the supported transition metal catalyst in a reaction for synthesizing high-carbon ketone through condensation coupling of alpha-H-containing ketone and alcohol. The preparation process of the supported transition metal catalyst comprises the steps that the porous catalyst carrier is added into a transition metal salt solution to be dissolved, left to stand, dried, roasted and reduced, and transition metal salt is selected from one or more of transition metal nitrate, transition metal formate, transition metal oxalate and transition metal acetate. The transition metal is selected from transition metal elements in the VIIB family, the VIII family, the IB family and the IIB family in the periodic table of chemical elements, the transition metal is non-noble metal, the raw materials of the catalyst are easy to obtain, and the preparation cost of the catalyst is low; in catalysis of condensation coupling reaction of alpha-H-containing ketone and small molecular alcohol, target high-carbon ketone can be obtained with high selectivity, additional solvents and hydrogen sources are not needed in the reaction, long-time stable operation can be realized, and the method has a good industrial application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention relates to the field of catalytic technology, and in particular to a preparation method of a supported transition metal catalyst, a supported transition metal catalyst and application thereof in the condensation coupling reaction of α-H-containing ketones and alcohols to synthesize high-carbon ketones. [Background technology]

[0002] Ketones can be used as excellent organic solvents and important organic chemical raw materials in the synthesis of spices, organic synthesis, and the synthesis of pharmaceutical intermediates. The synthesis methods of ketones in the prior art are limited, and the reaction process is generally cumbersome and has many by-products. For example, the corresponding alcohol can be used to prepare the ketones through oxidative dehydrogenation, and the ketones and aldehydes can be hydrogenated through aldol condensation reaction, but these methods have high production costs and generally low product selectivity. For example, U.S. Patent No. 4146581 has reported a method for preparing pentanone by condensation, dehydration, and hydrogenation of acetaldehyde and acetone in the presence of hydrogen, but the product components obtained by this method are complex, the selectivity of the target product is low, and high-pressure hydrogen is required to participate in the reaction, which places high demands on the reaction conditions.

[0003] The size of the ketone molecule affects its reactivity and the energy released during the reaction. Compared with small molecule ketones, high carbon ketones have a relatively large molecular structure and can achieve more complex and diverse chemical reactions. In the prior art, it has been disclosed that α-H-containing ketones react with other small molecule carbonyl compounds such as ketones and aldehydes containing active α-H to obtain condensation coupling products, which can be further prepared by dehydration and hydrogenation to obtain alkyl-grafted high carbon ketones. There are also alcohols used as condensation coupling reagents to couple with α-H-containing ketones to prepare high carbon ketones. In the prior art, the above-mentioned high carbon ketone reaction process needs to go through four steps of hydrogen borrowing (alcohol dehydrogenation to obtain small molecule carbonyl compounds containing active α-H), aldol condensation (the substrate contains α-H ketones), dehydration, hydrogenation, etc., which puts high demands on the design of the catalyst; the catalyst systems reported in the prior art include supported precious metal catalysts, homogeneous catalysts or composite oxide catalysts. For example, CN106732555A reports a Pd / C catalyst for the α-alkylation reaction of ketones and alcohols, but the solvent 1,4-dioxane is required to catalyze the reaction of acetophenone and n-butanol. CN111889105A discloses a bifunctional catalyst for the alkylation of methanol and butanone to prepare 3-pentanone, the catalyst composition includes 2-30% nickel oxide, 40-90% magnesium oxide, 10-30% aluminum oxide and 0-20% zinc oxide, the reaction temperature is 220-350°C, and the molar ratio of the raw material methanol / butanone is 5-15:1. CN110423190A and CN106905125A respectively report an iron complex and a cobalt complex catalyzing the α-alkylation reaction of ketones, the catalysts are obtained by the reaction of 4'-dimethylaminophenyl-2,2':6',2"-terpyridine with anhydrous ferrous chloride, and 2,2;6,2"-terpyridine with cobalt chloride. It is not difficult to find that these disclosed technologies all have problems such as expensive catalysts, complicated and harsh reaction conditions, and difficulty in product separation and catalyst recovery. [Summary of the invention]

[0004] To solve the above problems, the present invention provides a method for preparing a supported transition metal catalyst, a supported transition metal catalyst and application thereof in the synthesis of high-carbon ketones by condensation coupling of α-H-containing ketones and alcohols.

[0005] In a first aspect, the present invention provides a method for preparing a supported transition metal catalyst; the preparation steps include:

[0006] S1. dissolving at least one transition metal salt in water, wherein the transition metal salt is selected from one or more of transition metal nitrates, transition metal formates, transition metal oxalates, and transition metal acetates;

[0007] S2. Add the porous catalyst carrier to the solution obtained in step S1 and stir at room temperature. Mix until evenly mixed;

[0008] S3. The mixture obtained in step S2 is placed in an oven and dried at 80-110 ° C to constant weight;

[0009] S4. The dried product obtained in step S3 is heated to 250-390°C in a calcining device and calcined for 5-8h;

[0010] S5. The calcined product obtained in step S4 is heated to 250-450°C in a reaction apparatus and reduced in a reducing atmosphere for 2-8h to obtain a supported transition metal catalyst;

[0011] The molar ratio n1:n2:n3 of the transition metal salt, the porous catalyst carrier and the solvent water is 1:5:50≤n1:n2:n3≤1:20:100.

[0012] Preferably, the molar ratio n1:n2:n3 of the transition metal salt, the porous catalyst carrier and the solvent water is 1:8:60≤n1:n2:n3≤1:12:80.

[0013] Optionally, the heating rate in the roasting device in step S4 is 2-10°C / min, and the roasting temperature is preferably 300-350°C.

[0014] Optionally, in step S5, the heating rate in the reaction device is 2-10°C / min, and the reduction temperature is preferably 300-350°C.

[0015] Optionally, the transition metal in the transition metal nitrate and the transition metal acetate is selected from at least one of Mn, Ni, Co, Fe, Zn and Cu; preferably, the transition metal is selected from at least one of Ni, Co and Cu.

[0016] Preferably, the transition metal salt is selected from two or more of transition metal nitrates, transition metal formates, transition metal oxalates and transition metal acetates.

[0017] Optionally, the porous catalyst is selected from porous materials; preferably at least one of porous carbon materials, carbon nanotubes, alkaline earth oxides, aluminum oxide, silicon oxide, silicon aluminum oxide, and silicate; more preferably, the porous catalyst is selected from at least one of activated carbon and magnesium oxide.

[0018] More preferably, the reducing atmosphere is a H2 / N2 mixed gas flow; the volume ratio of H2 in the H2 / N2 mixed gas flow is 5%-50%.

[0019] In a second aspect, the present invention further provides a supported transition metal catalyst, which is prepared by the above catalyst preparation method.

[0020] Optionally, the supported transition metal catalyst includes any one of Ni5-Fe1 / AC, Ni2-Fe1 / AC, Ni5-Co1 / AC, Ni5-Cu1 / AC, Co5-Zn / AC, Mn5-Cu1 / AC, Ni5 / AC, Co2 / AC, Ni5-Fe1 / CNT, and Ni5-Fe1 / MgO.

[0021] In the third aspect, the present invention provides a catalytic synthesis method for high-carbon ketones. In a closed reaction device, the supported transition metal catalyst obtained by the above method is used as a reaction catalyst, and α-H-containing ketones and alcohols are used as reaction substrates; the high-carbon ketones are obtained by condensation coupling reaction at an initial pressure of normal pressure and a reaction temperature of 120 to 250°C.

[0022] Optionally, the alcohol is selected from at least one of aliphatic alcohols, aromatic alcohols, alicyclic alcohols or alcohols containing other heteroatom substituents; more preferably, the alcohol is selected from at least one of ethanol, n-propanol, isopropanol, ethylene glycol, phenylethyl alcohol, cyclohexanol and ethanolamine.

[0023] Optionally, the α-H-containing ketone is selected from at least one of aliphatic ketones, aromatic ketones, alicyclic ketones or ketones containing other heteroatom substituents; more preferably, the ketone is selected from at least one of acetone, butanone, pentanone, acetophenone, cyclohexanone and 1-amino-2-propanone.

[0024] Optionally, the molar ratio of the ketone to the alcohol is 1:2-2:1, and the feeding ratio of the ketone to the supported transition metal catalyst is 0.2-0.3 g of supported transition metal catalyst per 1 mol of ketone.

[0025] Optionally, the condensation coupling reaction can be carried out by a kettle reactor, a fixed bed or a fluidized bed process; preferably, the condensation coupling reaction is carried out by a continuous method with simultaneous feeding and discharging; preferably, the reaction temperature is 160-210°C and the reaction time is 30-300min.

[0026] The transition metal catalyst provided by the present invention can efficiently catalyze the condensation coupling reaction of ketones and small molecule alcohols to obtain target high-carbon ketones with high selectivity. In addition, the metal used in the catalyst is a non-precious metal, and the catalyst raw material used is easy to obtain, which significantly reduces the cost of the catalyst. When the catalyst of the present invention is used to catalyze the ketone-alcohol condensation reaction, no external solvent or high-pressure hydrogen is required, the reaction process is easy to implement, and the preparation method is simple; in addition, the catalytic condensation coupling conversion rate is high and the applicable alcohol categories are wide. The conversion rates of alcohols and ketones can be as high as 80% or more, respectively, and the selectivity of the target high-carbon ketone can be as high as 90% or more, and it can operate stably for a long time, and has a good industrial application prospect. [Specific implementation method]

[0027] In order to better understand the technical solution of the present invention, the embodiments of the present invention are described in detail below.

[0028] It should be clear that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0030] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0031] In the description of this specification, it is necessary to understand that the words such as "substantially", "approximately", "approximately", "about", "roughly", "substantially" and the like described in the claims and embodiments of the present invention refer to what can be generally recognized within a reasonable process operation range or tolerance range, rather than an exact value.

[0032] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited thereto.

[0033] A method for preparing a supported transition metal catalyst comprises the following preparation steps:

[0034] S1. dissolving at least one transition metal salt in water, wherein the transition metal salt is selected from one or more of transition metal nitrates, transition metal formates, transition metal oxalates, and transition metal acetates;

[0035] S2. Add the porous catalyst support to the solution obtained in step S1 and stir at room temperature until the mixture is uniform;

[0036] S3. The mixture obtained in step S2 is placed in an oven and dried at 80-110 ° C to constant weight;

[0037] S4. The dried product obtained in step S3 is heated to 250-390°C in a calcining device and calcined for 5-8h;

[0038] S5. The calcined product obtained in step S4 is heated to 250-450° C. in a reaction device and reduced in a H2 / N2 mixed gas flow for 2-8 h to obtain a supported transition metal catalyst.

[0039] The molar ratio n1:n2:n3 of the transition metal salt, the porous catalyst carrier and the solvent water is: 1:5:50≤n1:n2:n3≤1:20:100; preferably, 1:8:60≤n1:n2:n3≤1:12:80.

[0040] In step S4, the heating rate in the roasting device is 2-10°C / min, and the roasting temperature is preferably 300-350°C.

[0041] In step S5, the heating rate in the reaction device is 2-10°C / min, and the reduction temperature is preferably 300-350°C.

[0042] Preferably, the transition metal element in the transition metal salt is selected from the transition metal elements in Group VIIB, Group VIII, Group IB and Group IIB in the periodic table of chemical elements, and the transition metal is a non-precious metal. Optionally, the transition metal is selected from at least one of Mn, Ni, Co, Fe, Zn and Cu; preferably, the transition metal is selected from at least one of Ni, Co and Cu.

[0043] Preferably, the transition metal salt is selected from two or more of transition metal nitrates, transition metal formates, transition metal oxalates and transition metal acetates.

[0044] The transition metal used in the catalyst of the present invention is a non-noble metal, the catalyst raw material used is easily available, and the catalyst cost is significantly reduced.

[0045] Optionally, the porous catalyst carrier is selected from at least one of porous carbon materials, carbon nanotubes, alkaline earth oxides, aluminum oxide, silicon oxide, silicon aluminum oxide, and silicate; more preferably, the porous catalyst carrier is selected from at least one of porous carbon and magnesium oxide.

[0046] The connecting holes between the pores of the porous catalyst carrier are relatively small, and the catalyst is confined in the holes after being loaded, and is not easy to agglomerate, thereby significantly improving the life of the catalyst.

[0047] For example, refer to the following Examples 1-10:

[0048] Example 1

[0049] After dissolving nickel nitrate hexahydrate and ferric nitrate nonahydrate with water, add activated carbon, stir at room temperature for 7-10 hours, and place in an oven at 100°C to dry to constant weight. The molar ratio of nickel nitrate hexahydrate, ferric nitrate nonahydrate, activated carbon, and water is 5:1:50:320. After drying to constant weight, place in a muffle furnace for roasting, roast in an air atmosphere at 300°C for 6 hours, with a heating rate of 5°C / min, and then reduce at 400°C for 8 hours (heating rate of 5°C / min) in a 5% H2 / N2 mixed gas flow to obtain a catalyst, which is recorded as Ni5-Fe1 / AC.

[0050] Embodiment 2-6

[0051] The same method as in Example 1 was adopted to prepare the catalyst, but the transition metal nitrate and its ratio, and the reaction conditions were changed. The calcination temperatures were set to 300°C, 250°C, 350°C, 330°C, and 300°C, respectively; the heating rates were set to 5°C / min, 7°C / min, 9°C / min, 3°C / min, and 5°C / min, respectively, and the reduction temperatures were preferably 400°C, 300°C, 250°C, 450°C, and 400°C.

[0052] The obtained catalysts were respectively recorded as: Ni2-Fe1 / AC, Ni5-Co1 / AC, Ni5-Cu1 / AC, Co5-Zn1 / AC, Mn5-Cu1 / AC. For specific feed ratios, please refer to Table 1 below.

[0053] Embodiment 7-8

[0054] The same method and reaction conditions as in Example 1 for preparing the catalyst were adopted, but the catalyst carrier was changed to carbon nanotubes CNT and MgO as catalyst carriers. The obtained catalysts were respectively recorded as: Ni5-Fe1 / CNT and Ni5-Fe1 / MgO.

[0055] Examples 9-10

[0056] The same method and reaction conditions as those in Catalyst Preparation Example 1 were adopted, and a single transition metal nitrate was used as a substrate. The obtained catalysts were respectively recorded as: Ni5 / AC, Co2 / AC.

[0057] Table 1: Preparation of transition metal catalysts Substrate feed table

[0058]

[0059] In addition, the present invention also provides a catalytic synthesis method for high-carbon ketones. In a closed reaction device, the above-mentioned supported transition metal catalyst is used as a reaction catalyst, and α-H-containing ketones and alcohols are used as reaction substrates; the high-carbon ketones are obtained by condensation coupling reaction at an initial pressure of normal pressure and a reaction temperature of 120 to 250°C.

[0060] Optionally, the alcohol may be at least one selected from aliphatic alcohols, aromatic alcohols, alicyclic alcohols or alcohols containing other heteroatom substituents; preferably, the alcohol is at least one selected from ethanol, n-propanol, isopropanol, ethylene glycol, phenylethyl alcohol, cyclohexanol and ethanolamine.

[0061] Optionally, the α-H-containing ketone is selected from at least one of aliphatic ketones, aromatic ketones, alicyclic ketones or ketones containing other heteroatom substituents; more preferably, the ketone is selected from at least one of acetone, butanone, pentanone, acetophenone, cyclohexanone and 1-amino-2-propanone.

[0062] The reaction can be carried out by a kettle reactor, a fixed bed or a fluidized bed process. It is further preferred to use a continuous method with simultaneous feeding and discharging to carry out the reaction; the process operation steps can be further simplified to achieve mass industrial production.

[0063] Preferably, the molar ratio of the ketone to the alcohol is preferably in the range of 1:2-2:1, and the feed ratio of the ketone to the supported transition metal catalyst is preferably 0.2-0.3 g of catalyst per 1 mol of ketone.

[0064] Preferably, the condensation coupling reaction is carried out by a continuous method of simultaneous feeding and discharging; preferably, the reaction temperature is 160-210° C., and the reaction time is 30-300 min.

[0065] For example, please refer to the following condensation coupling reaction examples 11-31:

[0066] Condensation coupling reaction example 11

[0067] In a 100 ml high-pressure reactor, 0.05 g of catalyst Ni5-Fe1 / AC, 20 ml of ethanol and 20 ml of acetone were added in sequence and reacted at 175°C for 1.7 hours. During the reaction, the speed of the stirring group was maintained at 500 r / min. After the reaction, the gas chromatography analysis results showed that the conversion rate of ethanol was 92%, the conversion rate of acetone was 87%, and the selectivity of 2-pentanone was 83%.

[0068] Condensation coupling reaction examples 12-31

[0069] Using a method similar to that of Reaction Example 11, the reaction conditions and substrates were changed, and the composition of the product after the reaction was analyzed. The reaction conditions and catalytic performance results of the coupling reaction example are shown in Table 2 below:

[0070] Table 2. Reaction conditions and catalytic performance results of condensation coupling reaction examples

[0071]

[0072]

[0073] When the catalyst of the present invention is used to catalyze the ketone-alcohol condensation reaction, no external solvent or high-pressure hydrogen is required, the reaction process is easy to implement, and the preparation method is simple; in addition, the catalytic condensation coupling conversion rate is high and the applicable alcohol categories are wide, the conversion rates of alcohol and ketone can be as high as more than 80%, the selectivity of the target high-carbon ketone can be as high as more than 90%, and it can operate stably for a long time, and has a good industrial application prospect.

Claims

1. A method for preparing a supported transition metal catalyst, characterized in that: The method comprises the following preparation steps: S1. dissolving at least one transition metal salt in water, wherein the transition metal salt is selected from one or more of transition metal nitrates, transition metal formates, transition metal oxalates, and transition metal acetates; S2. Add the porous catalyst support to the solution obtained in step S1 and stir at room temperature until the mixture is uniform; S3. The mixture obtained in step S2 is placed in an oven and dried at 80-110 ° C to constant weight; S4. The dried product obtained in step S3 is heated to 250-390°C in a calcining device and calcined for 5-8h; S5. The calcined product obtained in step S4 is heated to 250-450°C in a reaction apparatus and reduced in a reducing atmosphere for 2-8h to obtain a supported transition metal catalyst; The molar ratio n1:n2:n3 of the transition metal salt, the porous catalyst carrier and the solvent water is 1:5:50≤n1:n2:n3≤1:20:

100.

2. The method for preparing the catalyst according to claim 1, characterized in that: The heating rate in the roasting device in step S4 is 2-10°C / min, and the roasting temperature is preferably 300-350°C.

3. The method for preparing the catalyst according to claim 1, characterized in that: The heating rate in the reaction device in step S5 is 2-10°C / min, and the reduction temperature is preferably 300-350°C.

4. The method for preparing the catalyst according to claim 1, characterized in that: The transition metal in the transition metal nitrate, transition metal formates, transition metal oxalates and transition metal acetates is selected from at least one of Mn, Ni, Co, Fe, Zn and Cu.

5. The method for preparing the catalyst according to claim 1, characterized in that: The transition metal salt is selected from two or more of transition metal nitrates, transition metal formates, transition metal oxalates, and transition metal acetates.

6. The method for preparing the catalyst according to claim 1, characterized in that: The porous catalyst carrier is selected from at least one of porous carbon materials, carbon nanotubes, alkaline earth oxides, silicon oxide, silicon aluminum oxide, and silicate.

7. The method for preparing the catalyst according to claim 1, characterized in that: The reducing atmosphere is a H2 / N2 mixed gas flow; the volume ratio of H2 in the H2 / N2 mixed gas flow is 5%-50%.

8. A supported transition metal catalyst, prepared by the method for preparing the catalyst according to any one of claims 1 to 7.

9. The supported transition metal catalyst according to claim 8, characterized in that The supported transition metal catalyst is any one of Ni5-Fe1 / AC, Ni2-Fe1 / AC, Ni5-Co1 / AC, Ni5-Cu1 / AC, Co5-Zn / AC, Mn5-Cu1 / AC, Ni5 / AC, Co2 / AC, Ni5-Fe1 / CNT, and Ni5-Fe1 / MgO.

10. A catalytic synthesis method of high-carbon ketones, characterized in that: In a closed reaction device, the supported transition metal catalyst described in any one of claims 8 to 9 is used as a catalyst, and α-H-containing ketones and alcohols are used as reaction substrates; a high-carbon ketone is obtained by condensation coupling reaction at an initial pressure of normal pressure and a reaction temperature of 120-250°C.

11. The catalytic synthesis method of high-carbon ketone according to claim 10, characterized in that: The alcohol is selected from at least one of aliphatic alcohols, aromatic alcohols, alicyclic alcohols or alcohols containing other heteroatom substituents.

12. The catalytic synthesis method of high-carbon ketone according to claim 10, characterized in that: The α-H-containing ketone is selected from at least one of aliphatic ketones, aromatic ketones, alicyclic ketones or ketones containing other heteroatom substituents.

13. The catalytic synthesis method of high-carbon ketones according to claim 10, wherein the molar ratio of the ketone to the alcohol is 1:2-2:1; and the feed ratio of the ketone to the supported transition metal catalyst is 0.2-0.3 g of the supported transition metal catalyst per 1 mol of ketone.

14. The catalytic synthesis method of high-carbon ketone according to claim 10, characterized in that: The condensation coupling reaction can be carried out by a kettle reactor, a fixed bed or a fluidized bed process; the condensation coupling reaction is carried out by a continuous method of simultaneous feeding and discharging; the reaction temperature is 160-210° C., and the reaction time is 30-300 min.

Citation Information

Patent Citations

  • Preparation of supported catalyst and preparation of 1,4-cyclohexanediol through hydroquinone hydrogenation in fixed bed

    CN113292396A

  • Preparation method of high-dispersion supported transition metal catalyst

    CN113509934A

  • Supported catalyst, preparation method thereof and method for preparing high-carbon ketone

    CN118204085A

  • Process for the preparation of methylisopropyl ketone and diethyl ketone

    EP0224218A1

  • Manufacture of higher ketones

    US4146581A

Cited By

  • Preparation method and application of monatomic catalyst for synthesizing spiro compound from diol and naphthenic ketone

    CN119368185A

  • Supported catalyst as well as preparation method and application thereof

    CN119680545A

  • Preparation method of supported carbon-based catalyst

    CN120861052A

  • Method for preparing bimetallic element loaded carbon catalyst through microwave-assisted hydrogen reduction

    CN120961158A

  • A method for preparing bimetallic carbon catalysts by microwave-assisted hydrogen reduction

    CN120961158B