Silicon-modified copper-zinc-zirconium catalyst as well as preparation method and application thereof

The silicon-modified copper-zinc zirconium catalyst was prepared by co-current precipitation method to reduce the aggregation of Cu and Zn species, increase the specific surface area and active sites of the catalyst, solve the problem of low activity of Cu-based catalysts and significantly improve CO2 conversion and methanol selectivity, suitable for industrial applications.

CN119016054APending Publication Date: 2024-11-26EAST CHINA UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410842137.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing Cu-based catalysts have low activity when catalyzing CO2 hydrogenation into methanol, and it is necessary to improve the catalytic activity of the catalyst.

Method used

Silicon-modified copper-zinc zirconium catalyst is prepared by co-current precipitation method, and an appropriate amount of silicon is introduced to reduce the aggregation degree of Cu and Zn species, and increase the specific surface area of ​​the catalyst and the exposed active sites.

Benefits of technology

The CO2 conversion rate and methanol selectivity were significantly improved, the CO2 conversion rate increased by 22.26%, and the methanol selectivity increased by 42.37%. The process was simple, the raw materials were cheap, and it was suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016054A_ABST
    Figure CN119016054A_ABST
Patent Text Reader

Abstract

The invention provides a silicon modified catalyst. The silicon modified catalyst comprises hydrated nitrate of copper, hydrated nitrate of zinc, hydrated nitrate of zirconium, sodium carbonate and hydrated silicate of sodium. The silicon-modified copper-zinc-zirconium catalyst with a large specific surface area is prepared by a parallel flow precipitation method. The aggregation degree of copper and zinc species in the catalyst is reduced by introducing a proper amount of silicon. Meanwhile, active sites exposed in the catalyst are increased due to the large specific surface area, so that the generation of methanol is greatly promoted. Compared with a copper-zinc-zirconium catalyst, the catalyst modified by a proper amount of silicon improves the conversion rate of carbon dioxide and the selectivity of methanol.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of chemical catalysis, and relates to a method for preparing a silicon-modified copper-zinc-zirconium catalyst with a large specific surface area, and is used for catalyzing carbon dioxide (CO 2 ) is hydrogenated to synthesize methanol (MeOH). Background Art

[0002] Currently, catalytic CO 2 Hydrogenation to synthesize methanol (MeOH) is one of the current research hotspots. This process can not only reduce CO 2 The concentration of MeOH can also be used to obtain high value-added chemicals. In industry, MeOH can be used as a raw material to synthesize chemical products such as dimethyl ether, dimethyl carbonate, and aromatics. At the same time, MeOH can not only be used as an energy carrier, but also can be directly used in fuel cells.

[0003] Among the many published patents, Cu-based catalysts are considered to be the most effective catalysts for catalyzing CO 2 The mainstream catalyst for hydrogenation to MeOH, but it still has problems such as low activity. It is often considered to introduce metal or non-metal additives into the Cu-based catalytic system to promote the dispersion of Cu species and thus improve the catalytic performance.

[0004] Patent application with publication number CN114602477A discloses a method for CO 2 Double-shell hollow copper-zinc-based catalyst for low-temperature preparation of MeOH. The introduction of alkaline earth metal promoter Ba is conducive to the increase of specific surface area and the formation of small Cu particles. -1 ·h -1 Under the test conditions, CO 2 The conversion was 11.8% and the MeOH selectivity was 79.2%.

[0005] The patent application with publication number CN117282441A discloses a Mn-promoted copper-zinc catalyst. The addition of metal Mn promotes the formation of zinc malachite crystals, inhibits the agglomeration of Cu and Zn species in the catalyst and the growth of metal Cu particles. The increase in exposed active sites promotes the rapid generation of MeOH. Under the same conditions, CO 2 The conversion rate increased by 2.59% and the MeOH selectivity increased by 27.71%.

[0006] Patent application with publication number CN113398929A discloses a Cu / TiO 2 The catalyst was formed by coprecipitation of Cu atoms into TiO 2 The lattice promotes the dispersion of active centers to improve the catalytic activity.

[0007] Therefore, the preparation of a high-performance catalyst is CO 2 The improvement of the dispersion of active species is of utmost importance in the process of preparing MeOH, which can be achieved by improving the dispersion of active species. Summary of the invention

[0008] The present invention aims to solve the problem of low activity of current Cu-based catalysts by introducing non-metallic additives to enhance the catalytic activity of the catalysts to prepare CO 2 Catalyst for hydrogenation to MeOH.

[0009] The main purpose of the present invention is to provide a silicon-modified catalyst, which comprises hydrated nitrate of copper, hydrated nitrate of zinc, hydrated nitrate of zirconium, sodium carbonate and hydrated silicate of sodium.

[0010] In some embodiments, the molar ratio of copper (Cu), zinc (Zn), zirconium (Zr), and silicon (Si) in the hydrated nitrate of copper, the hydrated nitrate of zinc, the hydrated nitrate of zirconium, and the hydrated silicate of sodium is 40-80:10-50:5-20:1.2-3.

[0011] In some embodiments, the molar ratio of Cu, Zn, Zr, and Si in the hydrated nitrate of copper, the hydrated nitrate of zinc, the hydrated nitrate of zirconium, and the hydrated silicate of sodium is 60:30:10:1.92.

[0012] In some embodiments, the hydrated nitrate of copper is copper nitrate trihydrate (Cu(NO 3 ) 2 ·3H 2 O), the hydrated nitrate of zinc is zinc nitrate hexahydrate (Zn(NO 3 ) 2 6H 2 O), the hydrated nitrate of zirconium is zirconium nitrate pentahydrate (Zr(NO 3 ) 4 ·5H 2 O) and the sodium hydrated silicate is sodium silicate nonahydrate (Na 2 SiO 3 9H 2 O).

[0013] In order to achieve the above object, the present invention also provides a method for preparing a silicon-modified catalyst, the method comprising the following steps:

[0014] S110: adding hydrated nitrate of copper, hydrated nitrate of zinc and hydrated nitrate of zirconium into water to obtain component A;

[0015] S120: adding sodium carbonate and sodium hydrated silicate into water to obtain component B;

[0016] S130: placing the component A and the component B in two dropping funnels respectively, and dropping them into a container containing water at 70° C. at the same time under vigorous stirring;

[0017] S140: controlling the dripping rate of the component A to be constant, and changing the dripping rate of the component B to control the pH of the mixed solution C to be 6.8-7.2;

[0018] S150: After the dropping is completed, stirring for 0.5 to 1.5 hours to obtain a mixed solution D;

[0019] S160: The mixed solution D is filtered and washed to ensure that no sodium ions remain, and dried in an oven for 10 to 15 hours, and then calcined at 300 to 500° C. for 3 to 7 hours to obtain a catalyst.

[0020] In some embodiments, the molar ratio of Cu, Zn, Zr, and Si in the hydrated nitrate of copper, the hydrated nitrate of zinc, the hydrated nitrate of zirconium, and the hydrated silicate of sodium is 40-80:10-50:5-20:1.2-3.

[0021] In some embodiments, the molar ratio of Cu, Zn, Zr, and Si in the hydrated nitrate of copper, the hydrated nitrate of zinc, the hydrated nitrate of zirconium, and the hydrated silicate of sodium is 60:30:10:1.92.

[0022] In some embodiments, the hydrated nitrate of copper is copper nitrate trihydrate (Cu(NO 3 ) 2 ·3H 2 O), the hydrated nitrate of zinc is zinc nitrate hexahydrate (Zn(NO 3 ) 2 6H 2 O), the hydrated nitrate of zirconium is zirconium nitrate pentahydrate (Zr(NO 3 ) 4 ·5H 2 O) and the sodium hydrated silicate is sodium silicate nonahydrate (Na 2 SiO 3 9H 2 O).

[0023] In some embodiments, the reaction temperature of the method is 200-250° C., the reaction pressure is 3-6 MPa, and the flow rate is 20-60 mL / min.

[0024] Based on the above, another object of the present invention is to provide a catalyst for catalyzing CO 2 Use of hydrogenation to synthesize MeOH.

[0025] Another object of the present invention is to provide a catalyst prepared according to the above method.

[0026] Compared with the prior art, the present invention prepares a silicon-modified copper-zinc-zirconium catalyst with a large specific surface area by a parallel flow precipitation method. The aggregation degree of Cu and Zn species in the catalyst is reduced by introducing an appropriate amount of silicon. At the same time, the large specific surface area increases the exposed active sites in the catalyst, which greatly promotes the generation of MeOH. Compared with the copper-zinc-zirconium catalyst, the catalyst CO modified by an appropriate amount of silicon has a higher specific surface area than the copper-zinc-zirconium catalyst. 2 The conversion rate and MeOH selectivity increased by 22.26% and 42.37% respectively. The catalyst raw materials are cheap, the design is simple, the operation is simple and the reaction environment is moderate, which is suitable for large-scale production and industrial use. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:

[0028] Figure 1a and 1b The scanning electron microscope (SEM) images of the catalyst prepared in Preparation Example 2 of the present invention and the catalyst prepared in Comparative Example 1 are shown respectively. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.

[0030] In one embodiment of the present invention, the steps for preparing the silicon-modified copper-zinc-zirconium catalyst with a large specific surface area are as follows:

[0031] Weigh 0.06 mol Cu, 0.03 mol Zn and 0.01 mol Zr hydrated nitrate and dissolve them in an appropriate amount of deionized water to obtain component A. Weigh 0.11 mol Na 2 CO 3 With 0.0012~0.003mol Na 2 SiO 3 9H 2O, dissolved in an appropriate amount of deionized water to obtain component B. The component A and the component B are placed in two constant pressure dropping funnels respectively, and are simultaneously dropped into a beaker containing 100 mL of deionized water at 70°C under vigorous stirring. The dropping rate of the component A is controlled to be constant, and the dropping rate of the component B is changed to control the pH of the mixed solution C to 7.0±0.2. After the dropping is completed, the solution is stirred and aged for 1 hour to obtain a mixed solution D. The mixed solution D is filtered and washed to ensure that there is no sodium ion (Na + After drying in an oven for 12 hours, the mixture was calcined at 400° C. for 5 hours to obtain the catalyst of the present invention.

[0032] The steps for preparing the catalyst for comparison are as follows:

[0033] Weigh 0.06 mol Cu, 0.03 mol Zn and 0.01 mol Zr hydrated nitrate and dissolve them in an appropriate amount of deionized water to obtain component A. Weigh 0.11 mol Na 2 CO 3 , dissolved in an appropriate amount of deionized water to obtain component B. Place the component A and the component B in two constant pressure dropping funnels respectively, and drip into a beaker containing 100 mL of deionized water at 70°C under vigorous stirring. Control the dripping rate of the component A to be constant, and change the dripping rate of the component B to control the pH of the mixed solution C to 7.0±0.2. After dripping, stir and age for 1 hour to obtain a mixed solution D. Filter and wash the mixed solution D to ensure that there is no Na + After drying in an oven for 12 hours, the catalyst was calcined at 400°C for 5 hours to obtain a catalyst for comparison.

[0034] The specific surface area and the dispersion degree of active Cu species corresponding to the catalyst obtained by the method of the present invention are different, thereby showing different catalytic performances.

[0035] The present invention is further described below in conjunction with specific embodiments.

[0036] The reagents used in the preparation examples of the present invention are shown in Table 1:

[0037] Table 1: Main preparation reagents

[0038]

[0039] The evaluation conditions of all preparation examples are shown in Table 2:

[0040] Table 2: Catalyst evaluation conditions

[0041]

[0042] a: The reaction pressure of Preparation Example 4 is 5.0 MPa, and the others are consistent with those described in the above table.

[0043] b: The flow rate of Preparation Example 5 is 25 mL / min, and the others are consistent with those described in the above table.

[0044] Preparation Example 1

[0045] Weigh 0.06 mol Cu, 0.03 mol Zn and 0.01 mol Zr hydrated nitrate and dissolve them in 100 mL deionized water to obtain component A. Weigh 0.11 mol Na 2 CO 3 With 0.0012mol Na 2 SiO 3 9H 2 O, dissolved in 110mL deionized water to obtain component B. Place the component A and the component B in two constant pressure dropping funnels respectively, and drip into a beaker containing 100mL deionized water at 70°C under vigorous stirring. Control the dripping rate of the component A to be constant, and change the dripping rate of the component B to control the pH of the mixed solution C to 7.0±0.2. After dripping, stir and age for 1 hour to obtain a mixed solution D. Filter and wash the mixed solution D to ensure that there is no Na + After drying in an oven for 12 hours, the catalyst was calcined at 400°C for 5 hours. Finally, the catalyst was tableted, crushed, and sieved to 40-60 mesh to obtain the catalyst E1 for evaluation.

[0046] Preparation Example 2

[0047] Weigh 0.06 mol Cu, 0.03 mol Zn and 0.01 mol Zr hydrated nitrate and dissolve them in 100 mL deionized water to obtain component A. Weigh 0.11 mol Na 2 CO 3 With 0.00192mol Na 2 SiO 3 9H 2 O, dissolved in 110mL deionized water to obtain component B. Place the component A and the component B in two constant pressure dropping funnels respectively, and drip into a beaker containing 100mL deionized water at 70°C under vigorous stirring. Control the dripping rate of the component A to be constant, and change the dripping rate of the component B to control the pH of the mixed solution C to 7.0±0.2. After dripping, stir and age for 1 hour to obtain a mixed solution D. Filter and wash the mixed solution D to ensure that there is no Na + After drying in an oven for 12 hours, the catalyst was calcined at 400°C for 5 hours. Finally, the catalyst was tableted, crushed, and sieved to 40-60 mesh to obtain the catalyst E2 for evaluation.

[0048] Preparation Example 3

[0049] Weigh 0.06 mol Cu, 0.03 mol Zn and 0.01 mol Zr hydrated nitrate and dissolve them in 100 mL deionized water to obtain component A. Weigh 0.11 mol Na 2 CO 3 With 0.003 mol Na 2 SiO 3 9H 2 O, dissolved in 110mL deionized water to obtain component B. Place the component A and the component B in two constant pressure dropping funnels respectively, and drip into a beaker containing 100mL deionized water at 70°C under vigorous stirring. Control the dripping rate of the component A to be constant, and change the dripping rate of the component B to control the pH of the mixed solution C to 7.0±0.2. After dripping, stir and age for 1 hour to obtain a mixed solution D. Filter and wash the mixed solution D to ensure that there is no Na + After drying in an oven for 12 hours, the catalyst was calcined at 400°C for 5 hours. Finally, the catalyst was tableted, crushed, and sieved to 40-60 mesh to obtain the catalyst E3 for evaluation.

[0050] Preparation Example 4

[0051] Weigh 0.06 mol Cu, 0.03 mol Zn and 0.01 mol Zr hydrated nitrate and dissolve them in 100 mL deionized water to obtain component A. Weigh 0.11 mol Na 2 CO 3 With 0.00192mol Na 2 SiO 3 9H 2 O, dissolved in 110mL deionized water to obtain component B. Place the component A and the component B in two constant pressure dropping funnels respectively, and drip into a beaker containing 100mL deionized water at 70°C under vigorous stirring. Control the dripping rate of the component A to be constant, and change the dripping rate of the component B to control the pH of the mixed solution C to 7.0±0.2. After dripping, stir and age for 1 hour to obtain a mixed solution D. Filter and wash the mixed solution D to ensure that there is no Na + After drying in an oven for 12 hours, the catalyst was calcined at 400°C for 5 hours. Finally, the catalyst was tableted, crushed, and sieved to 40-60 mesh to obtain the catalyst E4 for evaluation.

[0052] Preparation Example 5

[0053] Weigh 0.06 mol Cu, 0.03 mol Zn and 0.01 mol Zr hydrated nitrate and dissolve them in 100 mL deionized water to obtain component A. Weigh 0.11 mol Na 2 CO3 With 0.00192mol Na 2 SiO 3 9H 2 O, dissolved in 110mL deionized water to obtain component B. Place the component A and the component B in two constant pressure dropping funnels respectively, and drip into a beaker containing 100mL deionized water at 70°C under vigorous stirring. Control the dripping rate of the component A to be constant, and change the dripping rate of the component B to control the pH of the mixed solution C to 7.0±0.2. After dripping, stir and age for 1 hour to obtain a mixed solution D. Filter and wash the mixed solution D to ensure that there is no Na + After drying in an oven for 12 hours, the catalyst was calcined at 400°C for 5 hours. Finally, the catalyst was tableted, crushed, and sieved to 40-60 mesh to obtain the catalyst E5 for evaluation.

[0054] Comparative Example 1

[0055] Weigh 0.06 mol Cu, 0.03 mol Zn and 0.01 mol Zr hydrated nitrate and dissolve them in an appropriate amount of deionized water to obtain component A. Weigh 0.11 mol Na 2 CO 3 , dissolved in an appropriate amount of deionized water to obtain component B. Place the component A and the component B in two constant pressure dropping funnels respectively, and drip into a beaker containing 100 mL of deionized water at 70°C under vigorous stirring. Control the dripping rate of the component A to be constant, and change the dripping rate of the component B to control the pH of the mixed solution C to 7.0±0.2. After dripping, stir and age for 1 hour to obtain a mixed solution D. Filter and wash the mixed solution D to ensure that there is no Na + After drying in an oven for 12 hours, the catalyst was calcined at 400°C for 5 hours. Finally, the catalyst was tableted, crushed, and sieved to 40-60 mesh to obtain the catalyst E6 for evaluation.

[0056] Example 1: Comparison of catalytic activity of the catalyst prepared by the present invention and the catalyst prepared by comparative example 1

[0057] Catalysts E1 to E5 prepared in the present invention and catalyst E6 prepared in comparative example 1 were evaluated for catalytic activity. The specific evaluation process is as follows: 1.0000 g of 40-60 mesh catalyst was weighed on an analytical balance and loaded into the constant temperature zone of the reaction tube. N 2 The back pressure was increased to 0.35-0.5 MPa higher than the reaction pressure to check the air tightness of the reaction device. After the leak test, 20% H 2 / 80%N 2, program the temperature to 180℃, reduce for 4 hours, then heat to 250℃, reduce for 4 hours. After the reduction is completed, release the reducing gas. After the reaction system is cooled to 230℃, introduce the raw material gas to the required pressure to start the reaction.

[0058] The catalysts E1 to E3 and E6 correspond to catalysts that differ only in the content of the silicon additive. The results are shown in Table 3.

[0059] As shown in Table 3, there is a volcano-shaped relationship between the activity of the catalyst and the silicon content. The introduction of an appropriate amount of non-metallic additive silicon can greatly improve the activity of MeOH synthesis. 2 The conversion rate reached 19.28%, and the MeOH selectivity reached 60.92%.

[0060] Table 3: Catalytic activity of catalysts

[0061]

[0062] After optimizing the process parameters of the reaction system, it was found that as the pressure increased, CO 2 The conversion rate and MeOH selectivity increased to 21.17% and 67.20% (catalyst E4), respectively. 2 Hydrogenation to MeOH is a reaction in which the number of gas molecules decreases. According to Le Chatelier's principle, an increase in pressure is conducive to the continuous progress of the reaction. 2 , H 2 The residence time of the reaction intermediates in the catalytic system increases, and the conversion can be fully realized, so the catalytic activity is improved, CO 2 The conversion rate and MeOH selectivity reached 20.35% and 69.07% (catalyst E5), respectively.

[0063] Example 2: The catalyst prepared by the present invention has a relatively large specific surface area

[0064] The aggregation of active species in the catalysts E1 to E3 prepared by the present invention and the catalysts prepared in the comparative example was observed by SEM. As can be seen from Figure 1, a large amount of active species are aggregated in the catalyst prepared in comparative example 1 (i.e., catalyst E6), and after a small amount of silicon is introduced (i.e., catalyst E2 prepared in preparation example 2), the aggregation degree of active species is significantly reduced. This shows that the presence of an appropriate amount of silicon species can promote the dispersion of active species in the catalyst. At the same time, as can be seen from Table 4 below, the copper-zinc-zirconium catalyst modified with an appropriate amount of silicon can have a large specific surface area, promote the exposure of active sites, and accelerate the synthesis of MeOH.

[0065] Table 4: Specific surface area of ​​catalysts

[0066]

[0067] In summary, the silicon-modified catalyst of the present invention reduces the aggregation degree of Cu and Zn species in the catalyst by introducing an appropriate amount of silicon. At the same time, the large specific surface area increases the exposed active sites in the catalyst, which greatly promotes the generation of MeOH. Compared with the catalyst without the introduction of silicon, the catalyst modified with an appropriate amount of silicon can significantly improve the CO 2 Conversion rate and MeOH selectivity, which can effectively catalyze CO 2 Hydrogenation to synthesize MeOH.

[0068] The present invention has been described by the above-mentioned relevant embodiments, however, the above-mentioned embodiments are only examples for implementing the present invention. It must be pointed out that the disclosed embodiments do not limit the scope of the present invention. On the contrary, modifications and equivalent settings contained in the spirit and scope of the claims are all included in the scope of the present invention.

[0069] All publications, patents and patent applications mentioned in this specification are incorporated herein by reference in their entirety. The extent to which each individual publication, patent or patent application is specifically and individually indicated is incorporated herein by reference. In addition, any reference cited or indicated should not be construed as admitting that these references can be used as prior art of the present invention. The title part in this application is used in this article to make this specification easy to understand and should not be construed as a necessary limitation.

Claims

1. A silicon-modified catalyst, characterized in that: The catalyst includes hydrated nitrate of copper, hydrated nitrate of zinc, hydrated nitrate of zirconium, sodium carbonate and hydrated silicate of sodium.

2. The catalyst according to claim 1, characterized in that: The molar ratio of copper, zinc, zirconium and silicon in the hydrated nitrate of copper, the hydrated nitrate of zinc, the hydrated nitrate of zirconium and the hydrated silicate of sodium is 40-80:10-50:5-20:1.2-3.

3. The catalyst according to claim 2, characterized in that: The molar ratio of copper, zinc, zirconium and silicon in the hydrated nitrate of copper, the hydrated nitrate of zinc, the hydrated nitrate of zirconium and the hydrated silicate of sodium is 60:30:10:1.

92.

4. The catalyst according to claim 1, characterized in that: The hydrated nitrate of copper is copper nitrate trihydrate, the hydrated nitrate of zinc is zinc nitrate hexahydrate, the hydrated nitrate of zirconium is zirconium nitrate pentahydrate, and the hydrated silicate of sodium is sodium silicate nonahydrate.

5. A method for preparing a silicon-modified catalyst, characterized in that: The method The method comprises the following steps: S110: adding hydrated nitrate of copper, hydrated nitrate of zinc and hydrated nitrate of zirconium into water to obtain component A; S120: adding sodium carbonate and sodium hydrated silicate into water to obtain component B; S130: placing the component A and the component B in two dropping funnels respectively, and dropping them into a container containing water at 70° C. at the same time under vigorous stirring; S140: controlling the dripping rate of the component A to be constant, and changing the dripping rate of the component B to control the pH of the mixed solution C to be 6.8-7.2; S150: After the dropping is completed, stirring for 0.5 to 1.5 hours to obtain a mixed solution D; S160: The mixed solution D is filtered and washed to ensure that no sodium ions remain, and dried in an oven for 10 to 15 hours, and then calcined at 300 to 500° C. for 3 to 7 hours to obtain a catalyst.

6. The method according to claim 5, characterized in that: The molar ratio of copper, zinc, zirconium and silicon in the hydrated nitrate of copper, the hydrated nitrate of zinc, the hydrated nitrate of zirconium and the hydrated silicate of sodium is 40-80:10-50:5-20:1.2-3.

7. The method according to claim 6, characterized in that: The molar ratio of copper, zinc, zirconium and silicon in the hydrated nitrate of copper, the hydrated nitrate of zinc, the hydrated nitrate of zirconium and the hydrated silicate of sodium is 60:30:10:1.

92.

8. The method according to claim 5, characterized in that: The hydrated nitrate of copper is copper nitrate trihydrate, the hydrated nitrate of zinc is zinc nitrate hexahydrate, the hydrated nitrate of zirconium is zirconium nitrate pentahydrate, and the hydrated silicate of sodium is sodium silicate nonahydrate.

9. The method according to claim 5, characterized in that: The reaction temperature of the method is 200-250° C., the reaction pressure is 3-6 MPa, and the flow rate is 20-60 mL / min.

10. Use of the catalyst according to any one of claims 1 to 4 for catalytic hydrogenation of carbon dioxide to methanol.

11. A catalyst prepared by the method according to any one of claims 5 to 9.

Citation Information

Patent Citations

  • Cu / TiO2 catalyst for preparing methanol through CO2 catalytic hydrogenation and preparation method of Cu / TiO2 catalyst

    CN113398929A

  • Double-shell hollow copper-zinc-based catalyst for preparing methanol from CO2 at low temperature and preparation method thereof

    CN114602477A

  • Catalyst for preparing methanol through CO2 hydrogenation and preparation method thereof

    CN117282441A