Lanthanum-assisted phosphoric acid modified transition metal catalyst, preparation method and application of lanthanum-assisted phosphoric acid modified transition metal catalyst in catalytic oxidation of chlorine-containing volatile organic pollutants
By using lanthanum-assisted phosphoric acid-modified transition metal catalysts, the problems of catalyst poisoning and insufficient product selectivity were solved, achieving low-temperature and high-efficiency catalytic oxidation of chlorine-containing volatile organic pollutants, with excellent anti-poisoning performance and high selectivity.
Patent Information
- Application Number
- CN202411123031.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Existing catalysts are prone to poisoning by impurities such as chlorine and sulfur when treating chlorine-containing volatile organic pollutants, leading to catalyst deactivation, shortened service life, and insufficient product selectivity.
A lanthanum-assisted phosphoric acid-modified transition metal catalyst was prepared by co-precipitation and acid treatment. Lanthanum was doped into the transition metal oxide lattice to construct an acid-redox equilibrium system, which activated lattice oxygen and surface acidic sites, and optimized the mobility of active oxygen.
It achieves efficient catalytic oxidation of chlorine-containing volatile organic pollutants at low temperatures, exhibits good resistance to poisoning and product selectivity, extends catalyst life, and reduces energy consumption.
Smart Images

Figure CN119016073A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of air pollution control, and relates to a lanthanum-assisted phosphoric acid-modified transition metal catalyst and a preparation method thereof, and application thereof in catalytic oxidation of chlorine-containing volatile organic pollutants. Background Art
[0002] With the further development of modern industry, the problem of air pollution has become particularly prominent. In recent years, extreme air pollution events such as haze, photochemical smog and acid rain have occurred frequently, causing great harm to the environment and human health. Volatile organic compounds (VOCs) are fine particulate matter (PM 2.5 ) and ozone (O 3 ), and its efficient control is an important issue in the field of air pollution control at this stage.
[0003] VOCs generally refer to organic liquids and solids with a saturated vapor pressure greater than 70Pa at room temperature and a boiling point below 260°C at normal pressure. Such compounds are widely used in industrial fields such as packaging printing, automotive spraying, synthetic leather, and rubber recycling. Among them, chlorinated volatile organic compounds (CVOCs) are a type of organic pollutants that are highly toxic and difficult to degrade. They also have the characteristics of pollution persistence, bioaccumulation, and long-range migration. Such compounds are raw materials widely used in industrial production. Because of their stable properties, they are not easy to decompose and have strong toxicity. In industrial processes, if they are not handled properly, polychlorinated benzenes or even dioxins (PCDDs) and other more toxic pollutants may be generated. Once they enter the natural environment with waste gas and wastewater, they will accumulate in the human body and cause serious and lasting impacts on the ecological environment. With the restriction of total emissions and the improvement of emission standards, strengthening the end-of-pipe treatment of CVOCs has become a key link in pollution control in the absence of cleaner alternative products. At present, the commonly used disposal methods can be divided into two categories: non-destructive (physical adsorption, condensation, membrane separation, etc.) and destructive technology (direct combustion, catalytic combustion, biodegradation, etc.). Among them, catalytic combustion is widely used to treat low-concentration industrial waste gas due to its low energy consumption, easy operation and environmental friendliness.
[0004] However, in actual industrial production processes, catalyst deactivation due to chlorine and sulfur is a long-standing and common problem. Most industrial waste gases, such as those emitted from municipal solid waste incineration, steel smelting, and cogeneration, contain chlorine-containing substances (HCl, Cl 2 and CVOCs (such as chlorobenzene and dioxins) and sulfur dioxide (SO 2 These strongly coordinated impurities (Cl- and S) will inevitably poison the active sites of the catalyst, forming inert Mx Cl y 、M x O y Cl z and M x (SO 4 ) y Species, which greatly shortens the service life of the catalyst and greatly limits the industrial application of the catalyst. At the same time, inert chlorides promote the formation of toxic polychlorinated by-products, leading to serious secondary pollution. Therefore, the anti-poisoning ability of the catalyst under actual working conditions and the selectivity of the product determine the practical prospects of the catalyst. Summary of the invention
[0005] In order to overcome the problems of insufficient anti-poisoning ability and product selectivity of the catalyst in the prior art, the purpose of the present invention is to provide a lanthanum-assisted phosphoric acid-modified transition metal catalyst and a preparation method and application thereof in catalytic oxidation of chlorinated volatile organic pollutants. The lanthanum-assisted phosphoric acid-modified transition metal catalyst prepared by the method has good low-temperature activity, anti-poisoning performance and product selectivity, and realizes its environmentally friendly characteristics while achieving high catalytic efficiency, strong anti-poisoning ability and low by-product production.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing a lanthanum-assisted phosphoric acid-modified transition metal catalyst comprises the following steps:
[0008] reacting the precipitant solution with a solution containing a cobalt salt and a lanthanum salt to obtain a purple powder;
[0009] The purple powder is roasted to obtain a solid powder;
[0010] The solid powder is dispersed in a phosphoric acid solution, mixed evenly, separated, and dried to obtain a lanthanum-assisted phosphoric acid-modified transition metal catalyst.
[0011] Furthermore, the precipitant is sodium carbonate, sodium bicarbonate or ammonia water.
[0012] Furthermore, the mass ratio of the precipitant to the cobalt salt is 7.6-12.7:8.3-16.6.
[0013] Furthermore, the cobalt salt is cobalt nitrate, and the lanthanum salt is lanthanum nitrate.
[0014] Furthermore, the mass ratio of cobalt nitrate to lanthanum nitrate is 8.3-16.6:0.7-1.3.
[0015] Furthermore, the calcination temperature is 500-600°C and the time is 3-4h.
[0016] Furthermore, the concentration of the phosphoric acid solution is 0.1 mol / L, and the dispersion time is 40-50 minutes.
[0017] A lanthanum-assisted phosphoric acid-modified transition metal catalyst.
[0018] Application of a lanthanum-assisted phosphoric acid-modified transition metal catalyst in the catalytic decomposition of chlorinated volatile organic pollutants.
[0019] Furthermore, in the case of chlorobenzene reaction space velocity of 20000-30000 mL·h -1 ·g -1 , under the condition of oxygen concentration of 10-21%, the catalyst can achieve the degradation of chlorobenzene at 100-350℃.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention adopts a lanthanum-assisted phosphoric acid modification strategy, which utilizes the strong affinity of lanthanum for phosphate to avoid the conversion of active sites into inactive phosphates during phosphoric acid modification, thereby successfully constructing an "acid-redox" equilibrium system on the surface of the material. Lanthanum is doped into the lattice of transition metal oxides by coprecipitation, causing the lattice of transition metal oxides to be distorted, thereby activating lattice oxygen, generating a large number of oxygen vacancies on the surface, and optimizing the mobility of active oxygen species. Subsequently, during the phosphoric acid modification process, the lanthanum site-directedly anchors the phosphate, generating a rich Acidic sites (LaPO 4 ), the resulting catalyst has appropriate surface acidity and redox properties, successfully activating the synergistic effect between acidic sites and active sites. Compared with the traditional phosphoric acid modification strategy, the lanthanum-assisted phosphoric acid modification strategy not only generates rich The acid sites are further optimized, and the mobility of active oxygen is further optimized, achieving a balance between the catalyst surface acidity and redox performance through a convenient modification method. The metal elements in the composite metal oxide catalyst play independent and mutually influential roles and are effective degradation materials for chlorinated volatile organic pollutants.
[0022] The lanthanum-assisted phosphoric acid-modified catalyst prepared by the present invention has excellent low-temperature catalytic activity and outstanding anti-poisoning (Cl and SO 2 ) performance. At a reaction space velocity of 20000-30000 mL·h -1 ·g -1 Under the condition of oxygen concentration of 10-21%, 90% degradation of chlorobenzene in typical industrial CVOCs can be achieved at about 260°C, and the activity can be kept stable for 50 hours. In addition, at 300°C and the reaction space velocity of about 20000mL·h -1 ·g -1Under the conditions, 50 ppm SO 2 , within 30 hours, there was no deactivation. The catalyst has good low temperature activity and is resistant to poisoning (Cl and SO 2 ) and other advantages, and has important application prospects in the field of low-temperature purification of chlorinated volatile organic pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The lanthanum-assisted phosphoric acid-modified catalyst in the present invention is subjected to temperature-programmed reduction (H 2 -TPR) curve;
[0024] Figure 2 The lanthanum-assisted phosphoric acid modified catalyst in the present invention is subjected to temperature-programmed desorption (NH 3 -TPD) curve;
[0025] Figure 3 This is the element valence state distribution (XPS) curve of the lanthanum-assisted phosphoric acid-modified catalyst O1s in the present invention;
[0026] Figure 4 This is the activity test curve of the lanthanum-assisted phosphoric acid-modified catalyst in the present invention for catalytic degradation of chlorobenzene;
[0027] Figure 5 This is a stability test curve of the lanthanum-assisted phosphoric acid-modified catalyst catalyzing the degradation of chlorobenzene in the present invention;
[0028] Figure 6 The lanthanum-assisted phosphoric acid-modified catalyst of the present invention is used to catalyze the degradation of chlorobenzene to SO 2 Resistance test curve. DETAILED DESCRIPTION
[0029] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.
[0030] The present invention uses a multi-phase coprecipitation method and acid treatment to prepare a multifunctional lanthanum-assisted phosphoric acid-modified transition metal catalyst La-CoO for synergistically treating chlorinated volatile organic pollutants x-P. The present invention mainly uses a lanthanum-assisted phosphate modification strategy to directionally anchor phosphate groups on the surface lanthanum sites, and combines the doped lanthanum element to distort the lattice, thereby increasing the content of oxygen vacancies, activating the synergistic effect of active sites and acid sites, and improving its low-temperature oxidation activity and anti-poisoning ability. The metal elements in the composite metal oxide catalyst play independent and mutually influential roles and are effective degradation materials for chlorine-containing volatile organic pollutants. The specific steps are as follows:
[0031] (1) Dissolve 7.6-12.7 g of a precipitant (sodium carbonate, sodium bicarbonate or ammonia water) in 60-100 mL of deionized water and stir at 600-800 r / min for 30 min at room temperature until the precipitant is completely dissolved and a clear and transparent solution is formed;
[0032] (2) dissolving 8.3-16.6 g of cobalt nitrate in 80-120 mL of deionized water, stirring at 600-800 r / min for 30 min at room temperature until it is completely dissolved and a clear and transparent solution is formed;
[0033] (3) dissolving 0.7-1.3 g of lanthanum nitrate in the clear solution obtained in step (2), stirring at 600-800 r / min for 30 min at room temperature until it is completely dissolved and a clear and transparent solution is formed;
[0034] (4) adding the clarified solution obtained in step (1) dropwise to the solution obtained in step (3) at a rate of 10 drops / min, and stirring for 4 hours after the addition is complete to allow the solution to fully react;
[0035] (5) filtering the liquid obtained in step (4) under vacuum conditions, and washing with deionized water and anhydrous ethanol several times to obtain a purple powder, and then drying the obtained purple powder in an oven at 110° C. for 10-12 h until the obtained powder is dry;
[0036] (6) calcining the dried powder obtained in step (5) at 500-600° C. in a muffle furnace for 3-4 h to obtain a black solid powder;
[0037] (7) Re-dispersing 1 g of the black powder obtained in step (6) in 60 mL of 0.1 mol / L phosphoric acid solution and ultrasonically treating for 40-50 min;
[0038] (8) The solution obtained in step (7) is then filtered under vacuum conditions and washed with deionized water and anhydrous ethanol multiple times to obtain a black powder. The obtained black powder is then placed in a vacuum drying oven and dried at 60° C. for 10-12 h until the obtained powder is dry, thereby finally obtaining a catalyst with a high specific surface area.
[0039] The prepared catalyst is doped with lanthanum, making Co3 O 4 The crystal lattice is distorted, activating the lattice oxygen on the surface of the material, enhancing the fluidity of the active oxygen, and achieving efficient oxidation of the target pollutants.
[0040] The prepared catalyst is treated under acidic conditions so that the phosphate groups can be directionally anchored on the surface lanthanum sites, so the surface has abundant acidic sites.
[0041] The prepared catalyst belongs to composite metal oxides, and the catalytic effects of different metal oxides are independent and synergistic. Co in this system mainly provides low-temperature reduction active sites and achieves deep oxidation of target pollutants, while La mainly provides phosphate anchoring sites and promotes the transfer and removal of chlorine. The two metal oxides synergize with each other and promote the deep oxidation of chlorobenzene.
[0042] The application of the prepared catalyst in catalyzing the decomposition of chlorinated volatile organic pollutants is as follows: at a reaction space velocity of 20000 to 30000 mL·h -1 ·g -1 , under the condition of oxygen concentration of 10-21%, 90% degradation of chlorobenzene in typical industrial CVOCs can be achieved at around 260°C.
[0043] Example 1 Preparation of lanthanum-assisted phosphoric acid-modified catalyst using multiphase coprecipitation and acid treatment
[0044] Dissolve 15.98 g of cobalt nitrate and 1.29 g of lanthanum nitrate in 116 mL of deionized water, stir at 600 r / min for 30 min at room temperature until completely dissolved and a clear and transparent solution is formed; then add 100 mL of completely dissolved sodium carbonate solution containing 12.7 g dropwise, stir for 4 h after the addition is complete to allow the solution to fully react, then filter the resulting liquid under vacuum conditions, and wash with deionized water and anhydrous ethanol several times to obtain a purple powder.
[0045] The prepared purple powder was placed in an oven at 110° C. and dried for 12 h until the powder was dry; the dried powder was calcined in a muffle furnace at 500° C. for 4 h to obtain a black solid powder;
[0046] 1 g of black powder was redispersed in 60 mL of phosphoric acid solution with a concentration of 0.1 mol / L, and ultrasonically treated for 40 min. The obtained liquid was then filtered under vacuum conditions and washed with deionized water and anhydrous ethanol for multiple times to obtain black powder. The obtained black powder was then placed in a vacuum drying oven and dried at 60 ° C for 10 h until the obtained powder was dry, and finally a catalyst with a high specific surface area, namely La-CoO x -P oxide.
[0047] See also Figure 1It can be seen that the lanthanum-assisted phosphoric acid-modified catalyst has a reducible peak at 326°C, indicating that the material has excellent low-temperature reducibility and has great advantages in the field of catalytic oxidation.
[0048] See also Figure 2 It can be seen that the lanthanum-assisted phosphoric acid modified catalyst showed ammonia desorption peaks at 205 and 487 °C, indicating that the material has excellent weak acid and medium-strong acid properties, and has a good inhibitory effect on polychlorinated by-products during the catalytic oxidation of chlorinated volatile organic compounds.
[0049] See also Figure 3 , it can be seen that the surface of the lanthanum-assisted phosphoric acid-modified catalyst contains abundant surface lattice oxygen (529.6 eV) and surface adsorbed oxygen (531.0 eV), which can promote the deep oxidation of chlorinated volatile organic pollutants.
[0050] The catalyst prepared by the present invention has a large specific surface area (78.75m 2 ·g -1 ) and pore volume (0.176cm 3 ·g -1 ) can effectively promote the transmission of target pollutants on the surface of catalytic materials.
[0051] Example 2 Activity test and evaluation of lanthanum-assisted phosphoric acid-modified catalyst for catalytic degradation of chlorobenzene
[0052] The solid powder obtained in Example 1 was tableted and sieved (40-60 mesh), and 0.3 g of the sieved catalyst was accurately weighed. Chlorobenzene was used as the probe gas, the concentration of the reactant was controlled at 500 ppm, and the reaction space velocity was 20000 mL·h -1 ·g -1 Under the condition of oxygen concentration of 21%, the catalytic reaction activity of the catalyst at different temperatures (100, 150, 200, 250, 270, 290, 300 and 350° C.) was tested respectively, and the reaction products were monitored and analyzed by gas chromatography.
[0053] See also Figure 4 It can be seen that the lanthanum-assisted phosphoric acid-modified catalyst has good low-temperature catalytic performance at 260 °C and a reaction space velocity of about 20000 mL·h -1 ·g -1 Under these conditions, 90% chlorobenzene conversion can be achieved, which can basically be applied to the current industrial catalytic RCO catalytic reaction device and can achieve good results.
[0054] Example 3 Stability test of chlorobenzene degradation catalyzed by lanthanum-assisted phosphoric acid-modified catalyst
[0055] The solid powder obtained in Example 1 was pressed into tablets and sieved (40-60 mesh). 0.3 g of the sieved catalyst was accurately weighed and placed in the fixed bed of the evaluation device. Chlorobenzene was used as the probe gas. The concentration of the reactant was controlled at 500 ppm and the reaction space velocity was 20000 mL·h -1 ·g -1 The oxygen concentration was 21%, and the catalytic reaction activity of the catalyst was continuously tested at 260° C. The reaction products were monitored and analyzed by gas chromatography.
[0056] See also Figure 5 It can be seen that the lanthanum-assisted phosphoric acid modified catalyst has a reaction space velocity of about 20000 mL·h at 260 °C. -1 ·g -1 Under the above conditions, within 30 hours, the conversion rate of chlorobenzene by the catalytic material is maintained at about 90%, showing very excellent oxidation stability of chlorine-containing volatile organic compounds.
[0057] Example 4: Degradation of SO in Chlorobenzene Catalyzed by Lanthanum-Assisted Phosphoric Acid-Modified Catalyst 2 Resistance
[0058] The solid powder obtained in Example 1 was pressed into tablets and sieved (40-60 mesh), and 0.3 g of the sieved catalyst was accurately weighed. Chlorobenzene was used as the probe gas, and the concentration of the reactants was controlled at 500 ppm. 50 ppm of SO 2 , reaction space velocity is 20000mL·h -1 ·g -1 , the oxygen concentration was 21%, and the catalytic reaction activity of the catalyst at 300°C was continuously tested. The reaction products were monitored and analyzed by gas chromatography and in-situ online mass spectrometry.
[0059] See also Figure 6 It can be seen that the lanthanum-assisted phosphoric acid-modified catalyst has a high reaction temperature at 300 °C and a reaction space velocity of about 20000 mL·h -1 ·g -1 Under the conditions, 50 ppm SO 2 Within 30 hours, the conversion rate of chlorobenzene by the catalytic material remained at 100%, showing excellent resistance to SO 2 And anti-chlorine poisoning properties.
[0060] Example 5 Analysis of chlorobenzene intermediates catalytically degraded by lanthanum-assisted phosphoric acid-modified catalytic materials
[0061] The solid powder obtained in Example 1 was tableted and sieved (40-60 mesh), and 0.3 g of the sieved catalyst was accurately weighed. Chlorobenzene was used as the probe gas, the concentration of the reactants was controlled at 500 ppm, and the reaction space velocity was 20000 mL·h -1 ·g -1, the oxygen concentration was 21%, and the intermediate product production of the catalyst at different temperatures (100, 150, 200, 250, 270, 290, 300 and 350°C) was tested respectively. The reaction products were monitored and analyzed by gas chromatography and in-situ online mass spectrometry.
[0062] Example 6
[0063] 16.6 g of cobalt nitrate and 1.3 g of lanthanum nitrate were dissolved in 120 mL of deionized water, and stirred at 650 r / min for 30 min at room temperature until they were completely dissolved and a clear and transparent solution was formed; then 100 mL of a completely dissolved sodium bicarbonate solution containing 12.7 g was added dropwise, and after the addition was completed, it was stirred for 4 h to allow the solution to fully react. Then the resulting liquid was filtered under vacuum conditions, and washed several times with deionized water and anhydrous ethanol to obtain a purple powder.
[0064] The prepared purple powder was placed in an oven at 110° C. and dried for 12 h until the powder was dry; the dried powder was calcined in a muffle furnace at 500° C. for 4 h to obtain a black solid powder;
[0065] 1 g of black powder was redispersed in 60 mL of phosphoric acid solution with a concentration of 0.1 mol / L, and ultrasonically treated for 40 min. The resulting liquid was then filtered under vacuum conditions and washed several times with deionized water and anhydrous ethanol to obtain a black powder. The resulting black powder was then placed in a vacuum drying oven and dried at 60° C. for 10 h until the powder was dry, and finally a catalyst with a high specific surface area was obtained.
[0066] Example 7
[0067] 8.3 g of cobalt nitrate and 0.7 g of lanthanum nitrate were dissolved in 80 mL of deionized water, and stirred at 700 r / min for 30 min at room temperature until they were completely dissolved and a clear and transparent solution was formed; then 60 mL of a completely dissolved sodium bicarbonate solution containing 7.6 g was added dropwise, and after the addition was completed, the mixture was stirred for 4 h to allow the solution to fully react. The resulting liquid was then filtered under vacuum conditions and washed several times with deionized water and anhydrous ethanol to obtain a purple powder.
[0068] The prepared purple powder was placed in an oven at 110° C. and dried for 11 h until the powder was dry; the dried powder was calcined in a muffle furnace at 600° C. for 3 h to obtain a black solid powder;
[0069] 1 g of black powder was redispersed in 60 mL of phosphoric acid solution with a concentration of 0.1 mol / L, and ultrasonically treated for 50 min. The resulting liquid was then filtered under vacuum conditions and washed several times with deionized water and anhydrous ethanol to obtain a black powder. The resulting black powder was then placed in a vacuum drying oven and dried at 60° C. for 10 h until the powder was dry, and finally a catalyst with a high specific surface area was obtained.
[0070] Example 8
[0071] 14.3 g of cobalt nitrate and 1.2 g of lanthanum nitrate were dissolved in 100 mL of deionized water, and stirred at 600 r / min for 30 min at room temperature until they were completely dissolved and a clear and transparent solution was formed; then 60 mL of a 25% ammonia solution containing 10 g of the completely dissolved ammonia solution was added dropwise, and after the addition was completed, it was stirred for 4 h to allow the solution to react fully. Then the resulting liquid was filtered under vacuum conditions, and washed several times with deionized water and anhydrous ethanol to obtain a purple powder.
[0072] The prepared purple powder was placed in an oven and dried at 110° C. for 10 h until the powder was dry; the dried powder was calcined in a muffle furnace at 520° C. for 4 h to obtain a black solid powder;
[0073] 1 g of black powder was redispersed in 60 mL of phosphoric acid solution with a concentration of 0.1 mol / L, and ultrasonically treated for 45 min. The resulting liquid was then filtered under vacuum conditions and washed several times with deionized water and anhydrous ethanol to obtain a black powder. The resulting black powder was then placed in a vacuum drying oven and dried at 60° C. for 10 h until the powder was dry, and finally a catalyst with a high specific surface area was obtained.
[0074] Example 9
[0075] Dissolve 12.9 g of cobalt nitrate and 1 g of lanthanum nitrate in 90 mL of deionized water, stir at 800 r / min at room temperature for 30 min, until completely dissolved and a clear and transparent solution is formed; then add dropwise 80 mL of completely dissolved sodium carbonate solution containing 10 g, stir for 4 h after the addition is complete to allow the solution to react fully, then filter the resulting liquid under vacuum conditions, and wash with deionized water and anhydrous ethanol several times to obtain a purple powder.
[0076] The prepared purple powder was placed in an oven at 110° C. and dried for 12 h until the powder was dry; the dried powder was calcined in a muffle furnace at 570° C. for 3 h to obtain a black solid powder;
[0077] 1 g of black powder was redispersed in 60 mL of phosphoric acid solution with a concentration of 0.1 mol / L, and ultrasonically treated for 42 min. The resulting liquid was then filtered under vacuum conditions and washed several times with deionized water and anhydrous ethanol to obtain a black powder. The resulting black powder was then placed in a vacuum drying oven and dried at 60° C. for 10 h until the powder was dry, thereby finally obtaining a catalyst with a high specific surface area.
[0078] The present invention uses a lanthanum-assisted phosphoric acid modification strategy to successfully construct an "acid-redox" equilibrium system on the surface of a transition metal catalyst. On the basis of anchoring abundant acid sites on the surface, the low-temperature redox ability is further enhanced, the surface lattice oxygen is activated, the synergistic effect between the active sites and the acid sites is exerted, and the desorption of toxic species adsorbed on the surface of the material is promoted, thereby showing excellent low-temperature catalytic performance, product selectivity and anti-poisoning ability, and achieving environmentally friendly characteristics. The material preparation method of the present invention is simple, economical, and simple to operate. It can effectively degrade CVOCs under low temperature conditions, reduce the energy consumption of the reaction process, and realize the economic and environmentally friendly catalytic concept. It has important application prospects in the field of low-temperature purification of chlorinated volatile organic pollutants.
[0079] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.
[0080] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
Claims
1. A method for preparing a lanthanum-assisted phosphoric acid-modified transition metal catalyst, characterized in that: The following steps are involved: reacting the precipitant solution with a solution containing a cobalt salt and a lanthanum salt to obtain a purple powder; The purple powder is roasted to obtain a solid powder; The solid powder is dispersed in a phosphoric acid solution, mixed evenly, separated, and dried to obtain a lanthanum-assisted phosphoric acid-modified transition metal catalyst.
2. The method for preparing a lanthanum-assisted phosphoric acid-modified transition metal catalyst according to claim 1, characterized in that: The precipitant is sodium carbonate, sodium bicarbonate or ammonia water.
3. The method for preparing a lanthanum-assisted phosphoric acid-modified transition metal catalyst according to claim 1, characterized in that: The mass ratio of the precipitant to the cobalt salt is 7.6-12.7:8.3-16.
6.
4. The method for preparing a lanthanum-assisted phosphoric acid-modified transition metal catalyst according to claim 1, characterized in that: The cobalt salt is cobalt nitrate, and the lanthanum salt is lanthanum nitrate.
5. The method for preparing a lanthanum-assisted phosphoric acid-modified transition metal catalyst according to claim 4, characterized in that: The mass ratio of cobalt nitrate to lanthanum nitrate is 8.3-16.6:0.7-1.
3.
6. The method for preparing the lanthanum-assisted phosphoric acid-modified transition metal catalyst according to claim 1, characterized in that: The calcination temperature is 500-600°C and the time is 3-4h.
7. The method for preparing a lanthanum-assisted phosphoric acid-modified transition metal catalyst according to claim 1, characterized in that: The concentration of the phosphoric acid solution is 0.1 mol / L, and the dispersion time is 40-50 minutes.
8. A lanthanum-assisted phosphoric acid-modified transition metal catalyst prepared according to the method of any one of claims 1 to 7.
9. Use of a lanthanum-assisted phosphoric acid-modified transition metal catalyst prepared by the method according to any one of claims 1 to 7 in catalyzing chlorine-containing volatile organic pollutants.
10. The use according to claim 9, characterized in that: In chlorobenzene, the reaction space velocity is 20000~30000mL·h -1 ·g -1 , under the condition of oxygen concentration of 10-21%, the catalyst can achieve the degradation of chlorobenzene at 100-350℃.
Citation Information
Patent Citations
Low-temperature catalytic combustion eliminating method of volatile chloro aryl hydrocarbons
CN101767011A
Phosphorylated perovskite type catalyst as well as preparation method and application thereof
CN112604700A
Method for improving sintering resistance of cobalt oxide catalyst by lanthanum doping
CN115069259A
Process for low-temperature catalytically burning chlorinated aliphatics
CN1907545A
Catalyst, catalyst composition, method for producing catalyst, and method for removing volatile organic compound
JP2023060772A
Cited By
Phosphoric acid modified cobalt-manganese-aluminum solid solution catalyst, preparation method thereof and application of phosphoric acid modified cobalt-manganese-aluminum solid solution catalyst in synergistic removal of non-methane hydrocarbon