Catalyst as well as preparation method and application thereof

By performing multi-step treatment on the catalyst support to form a hollow structure, the problem of poor catalyst stability and dispersion of active components is solved, and the conversion rate of the cold hydrogenation reaction and the conversion rate of silicon tetrachloride are improved.

CN119016097APending Publication Date: 2024-11-26HUALU ENG & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411203032.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The catalysts used by domestic polysilicon manufacturers in the SiCl4 cold hydrogenation process have poor stability and poor dispersion of active components, resulting in a low conversion rate of the cold hydrogenation reaction.

Method used

By adding a precipitant to the catalyst support, calcining, reducing, carbonizing, calcining and etching treatments, a catalyst with a hollow structure is formed, thereby improving the stability of the catalyst and the dispersion of the active components.

Benefits of technology

The conversion rate of the cold hydrogenation reaction and the stability of the catalyst are improved, the dispersion of the active components is enhanced, and the conversion rate of silicon tetrachloride is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016097A_ABST
    Figure CN119016097A_ABST
Patent Text Reader

Abstract

The invention provides a catalyst and a preparation method and application thereof, and the preparation method of the catalyst comprises the following steps: 1) adding a precipitator into a system comprising a catalyst carrier and a metal source to obtain a first catalyst precursor; 2) sequentially carrying out first roasting treatment and reduction treatment on the first catalyst precursor to obtain a second catalyst precursor; 3) carbonizing a system comprising the second catalyst precursor and a carbon source to obtain a third catalyst precursor; 4) performing second roasting treatment on a system comprising the third catalyst precursor and a silicon source to obtain a fourth catalyst precursor; 5) performing etching treatment on the fourth catalyst precursor to obtain a fifth catalyst precursor; and 6) performing third roasting treatment on the fifth catalyst precursor to obtain the catalyst. According to the preparation method of the catalyst provided by the invention, the prepared catalyst is relatively high in stability and relatively good in dispersity of active components, and the conversion rate of a cold hydrogenation reaction can be increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polysilicon, and in particular relates to a catalyst and a preparation method and application thereof. Background Art

[0002] In recent years, with the increasing demand in the field of new energy, the global polysilicon production capacity has entered a period of rapid growth. At present, more than 85% of the world's polysilicon is produced by the modified Siemens method. The by-product SiCl4 is reduced to SiHCl3 with H2 and recycled. This process is called the hydrogenation of SiCl4, which is divided into two processes: cold hydrogenation and thermal hydrogenation. Thermal hydrogenation is the conversion of SiCl4 and H2 into SiHCl3 and HCl at a high temperature of 1200-1250℃, with a conversion rate of only 15-20%; cold hydrogenation is the addition of SiCl4, H2, silicon powder and catalyst to the fluidized bed reaction, and SiHCl3 is generated under the conditions of reaction temperature of 400-600℃ and pressure of 2-4MPa. Unlike thermal hydrogenation, which requires a large amount of heat to be provided for the reaction, cold hydrogenation greatly reduces the heat required for the reaction by introducing a catalyst, with low energy consumption and high reaction efficiency.

[0003] At present, domestic polysilicon manufacturers carry out SiCl4 cold hydrogenation process, and the catalysts used have the problems of poor stability and poor dispersion of active components, which leads to low conversion rate of cold hydrogenation reaction. Summary of the invention

[0004] The main purpose of the present invention is to provide a method for preparing a catalyst. The catalyst prepared by the preparation method has high stability and good dispersibility of active components, and can improve the conversion rate of cold hydrogenation reaction.

[0005] The present invention also provides a catalyst prepared by the above preparation method. The catalyst has high stability and good dispersibility of active components, and can improve the conversion rate of cold hydrogenation reaction.

[0006] The present invention also provides a method for preparing trichlorosilane. Since the catalyst is used in the preparation method, the conversion rate of the raw material can be improved.

[0007] In a first aspect, the present invention provides a method for preparing a catalyst, comprising the following steps:

[0008] 1) adding a precipitant to a system including a catalyst support and a metal source to obtain a first catalyst precursor;

[0009] 2) performing a first calcination treatment and a reduction treatment on the first catalyst precursor in sequence to obtain a second catalyst precursor;

[0010] 3) performing a carbonization treatment on a system including the second catalyst precursor and a carbon source to obtain a third catalyst precursor;

[0011] 4) performing a second calcination treatment on the system including the third catalyst precursor and the silicon source to obtain a fourth catalyst precursor;

[0012] 5) subjecting the fourth catalyst precursor to an etching treatment at 20-80° C. for 0.5-2 h to obtain a fifth catalyst precursor;

[0013] 6) subjecting the fifth catalyst precursor to a third calcination treatment at 650-1000° C. for 0.1-2 h to obtain the catalyst.

[0014] In the preparation method as described above, the catalyst carrier is porous carbon, and the porous carbon is obtained by subjecting a carbon source to a pyrolysis treatment at a pressure of 0.6-1 KPa and then subjecting the carbon source to a pore expansion treatment.

[0015] The carbonization treatment comprises the following steps: introducing a carbon source into the second catalyst precursor at a temperature of 600-1000°C for 0.1-2h, maintaining a mass space velocity of 0.01-10h -1 , maintain for 0.5-1h after the addition.

[0016] In the preparation method as described above, the temperature of the second calcination treatment is 200-500° C. and the time is 1-10 h.

[0017] In the preparation method as described above, the pH value of the system is adjusted to 8-12 after adding the precipitant.

[0018] In the preparation method as described above, the temperature of the reduction treatment is 200-400° C. and the time is 1-5 h.

[0019] The preparation method as described above, before subjecting the first catalyst precursor to the first calcination treatment, further comprises: subjecting the first catalyst precursor to an aging treatment at 40-80° C. for 1-3 hours.

[0020] In a second aspect, the present invention provides a catalyst prepared according to the above-mentioned preparation method.

[0021] In a third aspect, the present invention provides a method for preparing trichlorosilane, which is obtained by catalyzing silicon tetrachloride using the above catalyst.

[0022] The preparation method of trichlorosilane as described above comprises the following steps: at a temperature of 300-500°C and a pressure of 2.5-4MPa, hydrogen, silicon tetrachloride and silicon powder are introduced into a fluidized bed reactor fixed with the catalyst to carry out a gas-solid contact reaction to obtain the trichlorosilane.

[0023] The preparation method of the catalyst provided by the present invention coats the catalyst carrier with two layers, etches the silicon dioxide layer through a second calcination treatment, and adjusts the thickness of the carbon coating layer through a third calcination treatment, so that the catalyst finally forms a hollow structure, so that the catalyst has higher stability and better dispersion of active components, thereby improving the conversion rate of the cold hydrogenation reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the following briefly introduces the drawings required for use in the embodiments of the present invention or related technologies. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0025] Figure 1 A schematic diagram of a process for preparing a catalyst provided by the present invention;

[0026] Figure 2 The adsorption-desorption curve of the catalyst support prepared in Example 1 of the present invention;

[0027] Figure 3 The pore size distribution diagram of the catalyst carrier prepared in Example 1 of the present invention;

[0028] Figure 4 The adsorption-desorption curve of the catalyst support prepared in Example 2 of the present invention;

[0029] Figure 5 This is a pore size distribution diagram of the catalyst carrier prepared in Example 2 of the present invention;

[0030] Figure 6 The adsorption-desorption curve of the catalyst support prepared in Example 3 of the present invention;

[0031] Figure 7 This is a pore size distribution diagram of the catalyst carrier prepared in Example 3 of the present invention;

[0032] Figure 8 The adsorption-desorption curve of the catalyst support prepared in Example 4 of the present invention;

[0033] Fig. 9 This is the pore size distribution diagram of the catalyst carrier prepared in Example 4 of the present invention. DETAILED DESCRIPTION

[0034] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the embodiment of the present invention will be clearly and completely described below in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Figure 1 A schematic diagram of a process for preparing a catalyst provided by the present invention. Figure 1 As shown, in the first aspect, the present invention provides a method for preparing a catalyst, comprising the following steps:

[0036] 1) adding a precipitant to a system including a catalyst support and a metal source to obtain a first catalyst precursor;

[0037] 2) performing a first calcination treatment and a reduction treatment on the first catalyst precursor in sequence to obtain a second catalyst precursor;

[0038] 3) performing a carbonization treatment on a system including the second catalyst precursor and a carbon source to obtain a third catalyst precursor;

[0039] 4) performing a second calcination treatment on the system including the third catalyst precursor and the silicon source to obtain a fourth catalyst precursor;

[0040] 5) subjecting the fourth catalyst precursor to an etching treatment at 20-80° C. for 0.5-2 h to obtain a fifth catalyst precursor;

[0041] 6) subjecting the fifth catalyst precursor to a third calcination treatment at 650-1000° C. for 0.1-2 h to obtain the catalyst.

[0042] The method for preparing a catalyst of the present invention comprises the following processes: a system including a catalyst carrier and a metal source is subjected to a precipitation treatment, a first calcination treatment, a reduction treatment, a carbonization treatment, a second calcination treatment, an etching treatment and a third calcination treatment, and finally a porous core-shell hollow structure catalyst is prepared.

[0043] Specifically, in step 1), a precipitant is added to a system including a catalyst carrier and a metal source to obtain a first catalyst precursor. The metal source can be obtained by adding a metal soluble salt to deionized water to prepare a solution. The metal soluble salt is a transition metal soluble salt, preferably a soluble salt of copper, cobalt, and nickel. Optionally, the soluble salt of copper is at least one of copper sulfate, copper nitrate, copper chloride, and copper acetate; the soluble salt of nickel is at least one of nickel sulfate, nickel nitrate, nickel chloride, and nickel acetate; the soluble salt of cobalt is at least one of cobalt sulfate, cobalt nitrate, cobalt chloride, and cobalt acetate. The mass concentration of copper in the solution is 0.01-10wt%; the mass concentration of cobalt is 0.001-2wt%; and the mass concentration of nickel is 0.001-2wt%. The concentration of the salt solution affects the particle size of the precipitated particles. A concentrated solution is conducive to the formation of fine particles and is more conducive to the distribution of metals, but too high a concentration will lead to impurity adsorption and uneven precipitation. The catalyst carrier can be a non-soluble porous material, and can include at least one of silicon dioxide, porous carbon, silicon carbide, zeolite, magnesium oxide, zirconium oxide, and titanium dioxide. The system including the catalyst carrier and the metal source can be obtained by mixing the catalyst carrier with a solution containing a metal soluble salt, the mixing time is 1-5h, preferably 2-3h, and the temperature is 40-80°C, preferably 50-60°C. And the carrier and the solution can be fully mixed by ultrasound, stirring and other methods, and the solution is fully diffused to fill the pore structure of the carrier material. The precipitant is an alkaline precipitant, which can be at least one of sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate, potassium bicarbonate, potassium hydroxide, ammonium carbonate, ammonium bicarbonate, urea and ammonia water, and the mass concentration of the alkaline precipitant solution is 10-20wt%. When the precipitant is added, the metal active component will be precipitated on the surface of the carrier material as a surface active component, and precipitation will occur in the pores of the carrier material to form an intrapore active component, so as to achieve uniform distribution and loading of the metal active component in the carrier.

[0044] In step 2), the first catalyst precursor is subjected to a first calcination treatment and a reduction treatment in sequence to obtain a second catalyst precursor. Wherein, the first calcination treatment can be carried out in an oxygen-containing atmosphere, for example, air or oxygen, so that the metal active component is loaded in the carrier in the form of an oxide. The temperature of the first calcination treatment is 200-500°C, and the time is 1-10h. The reduction treatment can be carried out in a reducing atmosphere, and the reducing atmosphere refers to a gas with reducing ability for the metal component loaded on the carrier, which can be a gas such as hydrogen, carbon monoxide, ammonia, or a gas mixed with an inert gas in a molar ratio of 0.5-2:1. The inert gas can be a commonly used inert gas such as nitrogen and argon. Before the reduction treatment, the equipment can be purged with an inert gas for 0.5-2h for gas replacement, and then the first catalyst precursor can be subjected to a reduction treatment under a pressure of 0.1-0.4Mpa.

[0045] The present invention does not limit the equipment used for the reduction treatment, as long as it can introduce reducing gas and meet the reduction temperature and pressure, for example, a tubular furnace or a fixed bed reactor.

[0046] In step 3), the system including the second catalyst precursor and the carbon source is carbonized to obtain a third catalyst precursor. The carbon source may be at least one of asphaltene, coal, coal tar, coal tar fraction, and biomass; preferably asphaltene. The purpose of the carbonization treatment is to form a carbon coating layer on the surface of the second catalyst precursor with the carbon source to protect the active metals loaded in the catalyst carrier, to avoid the wear of the catalyst particles during use, causing the active components, especially the surface active components, to fall off, thereby affecting the stability and service life of the catalyst.

[0047] In step 4), a second calcination treatment is performed on the system including the third catalyst precursor and the silicon source to obtain a fourth catalyst precursor. The silicon source may be silicon tetrachloride. Before the second calcination treatment, the third catalyst precursor may be purged with a mixed gas of water vapor and nitrogen. The treatment time is 5-30 min, the pressure is 0.1-0.4 MPa, the temperature is 100-200 ° C, the molar ratio of water vapor to nitrogen is 1:1-10, preferably 1:4-6, and the space velocity is ≥10h -1 (Calculated based on water vapor plus nitrogen). Then introduce silicon tetrachloride and nitrogen, the treatment time is 1-60min, the pressure is 0.1-0.4MPa, the temperature is 60-80℃, the molar ratio of silicon tetrachloride gas to nitrogen is 1:0.1-50, preferably 1:1-10, the space velocity is ≥100h -1 (calculated based on nitrogen plus silicon tetrachloride), silicon tetrachloride can absorb water to form silicic acid. Then, a second calcination treatment is performed under a nitrogen atmosphere to obtain a fourth catalyst precursor. The pressure of the second calcination treatment is 0.1013-0.4MPa; the nitrogen space velocity is ≥100h -1 After the second calcination treatment, the silicic acid is dehydrated, and a silicon dioxide layer is coated on the outer surface of the third catalyst precursor.

[0048] In step 5), the fourth catalyst precursor is etched at 20-80°C for 0.5-2h to obtain a fifth catalyst precursor. Wherein, the etching treatment uses an aqueous solution of sodium hydroxide and / or potassium hydroxide, and the molar concentration of the solution is 0.5-0.6mol / L. The etching treatment can be carried out in an alkaline vessel with sufficient stirring, such as maintaining a stirring speed of 500-1000r / min in a polytetrafluoroethylene beaker. The purpose of the etching treatment in the present invention is to remove the silicon dioxide layer coated on the pores of the catalyst carrier to expose the coated carbon layer, so that after the subsequent removal of the carbon layer at the pores of the catalyst carrier, the active components in the pores are exposed, and the catalytic effect of the active components in the pores is not affected. In the present invention, the concentration of the alkali solution for etching treatment and the temperature and time of the etching treatment are controlled within a suitable range, which can avoid the dissolution of the silicon dioxide layer due to excessive etching, and can also avoid insufficient etching, resulting in insufficient exposure of the active components in the pores, resulting in a decrease in the activity of the catalyst. After the etching treatment, the fifth catalyst precursor can be filtered, washed to neutrality, and dried, wherein the drying temperature is 100-200° C., preferably 120-150° C., and the drying time is 4-12 hours, preferably 6-8 hours.

[0049] In step 6), the fifth catalyst precursor is subjected to a third calcination treatment at 650-1000°C for 0.1-2h, which can change the pore size distribution of the catalyst and achieve the formation of a hollow structure. That is, on the one hand, the thickness of the carbon coating layer coated on the surface active component can be adjusted so that the surface active component can be fully exposed to play a catalytic role, and can adhere to the surface of the catalyst carrier and will not fall off during the reaction; on the other hand, the carbon coating layer coated on the pores of the catalyst carrier can be removed to expose the active components in the pores without affecting the catalytic effect of the active components in the pores. Controlling the temperature of the third calcination treatment to 650-1000°C and the time to 0.1-2h can avoid completely removing the carbon coating layer, making the surface active components easy to fall off; and can also avoid insufficient removal of the carbon coating layer, which cannot completely expose the surface active components and the active components in the pores to play their catalytic role. Optionally, an activated gas, such as water vapor, CO2 and O2, can be introduced into the third calcination treatment process. Specifically, the fifth catalyst precursor is placed in a reactor, and an inert gas is introduced for 10-30 min at a space velocity of 1-100 h -1 , remove oxygen, heat to 650-1000°C at a heating rate of 1-20°C, introduce activation gas, maintain for 10-100min, the mass ratio of activation gas to the fifth catalyst precursor is 1-10:1, after the reaction is completed, introduce inert gas to cool to room temperature to obtain the catalyst.

[0050] The present invention does not limit the reactor used in the third calcination treatment, as long as it can pass the activated gas and meet the temperature and pressure of the third calcination treatment, for example, a tubular furnace or a fixed bed reactor.

[0051] The preparation method of the catalyst of the present invention is to coat the catalyst carrier with two layers, etch the silicon dioxide layer through an etching treatment, adjust the thickness of the carbon coating layer through a third calcination treatment, and finally form a hollow structure of the catalyst, so that the catalyst has higher stability and better dispersion of active components, thereby improving the conversion rate of the cold hydrogenation reaction.

[0052] In some embodiments of the present invention, the catalyst carrier is porous carbon, and the porous carbon is obtained by subjecting a carbon source to a pyrolysis treatment at a pressure of 0.6-1 KPa and then subjecting the carbon source to a pore expansion treatment.

[0053] Specifically, the carbon source is subjected to pyrolysis treatment under an inert atmosphere and negative pressure to form a pore structure, part of which is formed by structural fracture and part of which is formed by the escape of volatile components. Different pyrolysis methods form different pore structures, and their morphology will affect the distribution of active components of the catalyst. Optionally, the negative pressure can be 0.6-1kPa; the inert atmosphere can be a commonly used inert gas such as nitrogen and argon; the carbon source is a high-carbon, low-hydrogen substance, which can be at least one of asphaltene, coal, coal tar, coal tar fraction, and biomass; wherein the coal tar fraction contains at least one of naphthalene oil, wash oil, and anthracene oil.

[0054] The formed pore structure is then subjected to pore expansion treatment to obtain porous carbon as a catalyst carrier. In one embodiment, the pore expansion treatment is performed by gas activation method to expand the formed pore structure and change its pore size distribution. In the gas activation method, at a certain temperature, the activated gas weakly oxidizes the carbon, thereby changing the morphology of the pore structure. Optionally, the activated gas can be at least one of water vapor, CO2, O2, and flue gas. In another embodiment, the pore expansion treatment is performed by chemical activation method to expand the formed pore structure and change its pore size distribution. The chemical activation method is to activate the formed pore structure with a chemical activator at a certain temperature to change the specific surface area of ​​the pore structure. The chemical activator can be at least one of caustic potash, potassium carbonate, caustic soda, sodium carbonate, zinc chloride, and nitric acid.

[0055] The present invention does not limit the equipment used in the gas activation method, as long as it can pass the activation gas and meet the activation temperature, for example, a tubular furnace, a fixed bed reactor.

[0056] The present invention does not limit the equipment used in the chemical activation method, as long as the chemical activating agent can be introduced and the activation temperature is met, for example, a tubular furnace or a fixed bed reactor.

[0057] In some embodiments of the present invention, the temperature of the pyrolysis treatment is 500-1000° C. and the time is 1-5 h.

[0058] In the present invention, the temperature can be raised to 500-1000° C. at a heating rate of 1-20° C. / min, and the temperature is maintained for 1-5 hours for pyrolysis treatment.

[0059] In the present invention, the temperature and time of the pyrolysis treatment are controlled, so that the pyrolysis treatment of the carbon source can be more complete, which is beneficial to the formation of a pore structure. When used as a catalyst carrier, the active component can be better dispersed.

[0060] In some embodiments of the present invention, the temperature of the hole expansion treatment is 650-1000° C. and the time is 0.5-5 h.

[0061] In one embodiment, the pore expansion treatment of the present invention can place the pore structure formed by the carbon source in a reactor, introduce an inert gas for 10-30 minutes, and maintain a space velocity of 1-100h -1 , remove oxygen, heat to 650-1000°C at a heating rate of 1-20°C / min, introduce activation gas, and maintain for 0.5-5h. The mass ratio of activation gas to pore structure is 1-10:1. After the reaction is completed, introduce inert gas to cool to room temperature to obtain porous carbon, i.e., catalyst carrier.

[0062] In another embodiment, the pore expansion treatment of the present invention can be performed by fully mixing the pore structure formed by the carbon source with the chemical activator and placing it in a reactor, wherein the mass ratio of the chemical activator to the pore structure is 1-10:1, and an inert gas is introduced for 10-30 minutes, and the space velocity is maintained at 1-100h -1 , remove oxygen, heat up to 650-1000°C at a heating rate of 1-20°C / min, maintain for 0.5-5h, and after the reaction is completed, introduce inert gas and cool to room temperature to obtain porous carbon, i.e., catalyst carrier.

[0063] In the present invention, the temperature and time of the pore expansion treatment are controlled so that the obtained catalyst carrier has a suitable pore size and pore size distribution, and the dispersibility of the active components can be further improved.

[0064] In some embodiments of the present invention, the carbonization treatment comprises the following process: introducing a carbon source into the second catalyst precursor at a temperature of 600-1000°C for 0.1-2h, maintaining a mass space velocity of 0.01-10h -1 , maintain for 0.5-1h after the addition.

[0065] In this embodiment, N2 can be introduced during the introduction of the carbon source to make the air velocity ≥ 1h -1, pushing the carbon source into the equipment for carbonization. After the carbon source is introduced, the temperature in the equipment is maintained at 600-1000℃ for 0.5-1h, so that the carbon source can be fully coated on the surface of the carrier loaded with active components to form a uniform carbon coating. Controlling the amount and time of the carbon source introduction can make the thickness of the formed carbon coating appropriate. During the carbonization process, the active component changes from adhering to the surface of the carrier to being embedded in the carbon coating, which ensures the stability of the active component and does not require bonding materials.

[0066] The carbonization process of the present invention can form a uniform carbon coating layer on the surface of the catalyst, thereby improving the stability of the active components in the catalyst and further improving the conversion rate of the cold hydrogenation reaction.

[0067] In some embodiments of the present invention, the temperature of the second calcination treatment is 200-500° C. and the time is 1-10 h.

[0068] In the present invention, the temperature of the second calcination treatment is 200-500°C, preferably 300-400°C; the time is 1-10h, preferably 2-5h. The outer surface of the third catalyst precursor can be coated with a layer of silicon dioxide, that is, the silicic acid can be dehydrated to form silicon dioxide. The brittle carbon layer can be further protected to prevent the carbon layer from falling off during the reaction, thereby causing the active component to fall off.

[0069] In some embodiments of the present invention, the pH value of the system is adjusted to 8-12 after adding the precipitant.

[0070] It can be understood that the precipitant added to the system including the catalyst carrier and the metal source in the present invention is an alkaline precipitant, which can simultaneously adjust the pH value of the system.

[0071] In the present invention, after adding the precipitant, the pH value of the system is adjusted to 8-12, preferably 9-10. The particle size of the precipitated particles is controlled by the crystal nucleus growth rate and the crystal nucleus generation rate. The faster the crystal nucleus generation rate, the smaller the particle size of the generated particles. Increasing the pH value will accelerate the formation of precipitated particles, increase the generation rate, and reduce the growth rate. By adjusting the pH value, the particle size of the active component loaded on the carrier can be regulated. Since there is a structure-activity relationship between the particle size of the active component and the catalyst reaction performance, the performance of the catalyst can be regulated by adjusting the pH value of the system.

[0072] The pH value of the regulating system in the present invention is 8-12, which is within a suitable range, so that the particle size of the active component loaded on the catalyst carrier can be suitable, so that the catalyst has better reaction activity and the conversion rate of the cold hydrogenation reaction can be improved.

[0073] In some embodiments of the present invention, the reduction treatment is carried out at a temperature of 200-400° C. and for a time of 1-5 h.

[0074] In the present invention, the temperature of the reduction treatment is controlled to be 200-400°C and the time is 1-5h. Within a suitable range, the active components loaded on the carrier can be reduced to a relatively stable valence state, which can further improve the stability of the active components of the catalyst.

[0075] In some embodiments of the present invention, before the first calcination treatment of the first catalyst precursor, the method further comprises: subjecting the first catalyst precursor to an aging treatment at 40-80° C. for 1-3 hours.

[0076] In the present invention, the temperature for aging the first catalyst precursor is 40-80° C., preferably 50-60° C., and the aging time is 1-3 hours, preferably 2-3 hours. During the aging process, the formed fine precipitate particles dissolve and redeposit, and impurities dissolve into the solution to obtain a relatively uniform precipitate of particles, so as to form a catalyst precursor with a relatively stable structure.

[0077] After the aging treatment, the catalyst precursor can be filtered to obtain a filter cake, which can be washed with water until neutral and dried at a temperature of 80-120° C., preferably 100-120° C., for 4-12 h, preferably 6-8 h.

[0078] The aging treatment in the present invention can make the formed precipitated particles more uniform, which is beneficial to the subsequent formation of a catalyst with a stable structure.

[0079] In a second aspect, the present invention provides a catalyst prepared according to the above-mentioned preparation method.

[0080] The catalyst of the present invention is prepared by the above-mentioned preparation method, so the catalyst has high stability and good dispersibility of active components, and can improve the conversion rate of cold hydrogenation reaction.

[0081] In a third aspect, the present invention provides a method for preparing trichlorosilane, which is obtained by catalyzing silicon tetrachloride using the above catalyst.

[0082] The method for preparing trichlorosilane in the present invention uses the above catalyst to catalyze silicon tetrachloride to obtain it, so the conversion rate of silicon tetrachloride is relatively high.

[0083] In some embodiments of the present invention, the method for preparing trichlorosilane comprises the following steps: at a temperature of 300-500° C. and a pressure of 2.5-4 MPa, hydrogen, silicon tetrachloride and silicon powder are introduced into a fluidized bed reactor fixed with the catalyst to carry out a gas-solid contact reaction to obtain the trichlorosilane.

[0084] In the present invention, the catalyst prepared as above can be first fixed in a fluidized bed reactor, and then the raw materials hydrogen, silicon tetrachloride and silicon powder are introduced into the fluidized bed reactor. At a temperature of 300-500° C. and a pressure of 2.5-4 MPa, silicon tetrachloride is in a gaseous state, so a gas-solid contact reaction occurs in the fluidized bed reactor to obtain trichlorosilane.

[0085] Optionally, before the raw materials are introduced into a fluidized bed reactor with a fixed catalyst for gas-solid contact reaction, an inert gas, such as nitrogen, is first introduced into the fluidized bed reactor to replace gases such as oxygen and carbon dioxide in the fluidized bed reactor, so that there is no gas in the fluidized bed reactor that affects the gas-solid contact reaction.

[0086] In the present invention, by using the above catalyst to catalyze silicon tetrachloride to obtain trichlorosilane, the preparation method can be simple and easy, and the raw material conversion rate is high.

[0087] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0088] Example 1

[0089] The preparation method of trichlorosilane of the present embodiment comprises the following steps:

[0090] 1) Add 7g of copper chloride (chemical formula CuCl2·2H2O), 1g of nickel chloride (chemical formula NiCl2·6H2O), and 1g of cobalt chloride (chemical formula CoCl2·6H2O) into 60mL of deionized water; after mixing, place the mixture in an oil bath at a constant temperature of 80°C and mix with ultrasonic vibration for 30min to fully dissolve the solute to obtain a salt solution;

[0091] 2) The asphaltene was heated to 800°C at a rate of 5°C / min under a nitrogen atmosphere at a pressure of 1 KPa (denoted as pressure 1) and kept warm for 2 hours to obtain pyrolytic carbon; under the temperature condition of 800°C, KOH was added in a mass ratio of KOH:pyrolytic carbon = 1:2, and after activation for 10 minutes, porous carbon was obtained after washing and drying at 120°C for 6 hours as a catalyst carrier;

[0092] 3) adding 10 g of the catalyst carrier to the prepared salt solution, stirring at 80° C. with a magnetic stirrer at a speed of 1000 r / min for 2 h to fully mix the mixture and obtain a suspension; adjusting the pH value of the suspension to 10 with ammonia water so that the precipitated metal is fully distributed on the catalyst carrier, allowing the suspension to stand for aging at 60° C. for 3 h, filtering to obtain a filter cake, washing with deionized water until neutral, and drying at 120° C. for 6 h to obtain a first catalyst precursor;

[0093] 4) After the first catalyst precursor was subjected to a first calcination treatment at 400° C. for 3 h, it was placed in a fixed bed reactor and purged with nitrogen at room temperature and pressure for 1 h at a flow rate of 50 mL / min, and then a mixture of hydrogen and nitrogen was introduced at a set temperature of 300° C. at a flow rate of 50 mL / min, and reduced for 2 h to obtain a second catalyst precursor;

[0094] 5) N2 was introduced into the second catalyst precursor at a flow rate of 300 mL / min and a temperature of 800°C, which was recorded as temperature 1. Asphaltene was introduced for 40 min, which was recorded as time 1. The space velocity was maintained at 3 h. -1 , the addition is completed and maintained for 1 hour to obtain a third catalyst precursor;

[0095] 6) At 120°C and normal pressure, a mixture of water vapor and nitrogen was introduced for 10 min, with the flow rates of nitrogen 5 mL / min and water vapor 1 mL / min, respectively, so that the catalyst precursor B absorbs a certain amount of water vapor; at 70°C and normal pressure, a mixture of silicon tetrachloride and nitrogen was introduced for 20 min, with nitrogen 100 mL / min and silicon tetrachloride (gas) 20 mL / min; at normal pressure, the temperature was raised to 300°C at a rate of 5°C / min, recorded as temperature 2, and a secondary calcination treatment was performed for 3 h, recorded as time 2, with a nitrogen flow rate of 50 mL / min, to obtain a fourth catalyst precursor;

[0096] 7) placing the fourth catalyst precursor in a NaOH solution for alkaline etching, the solution concentration is 0.5 mol / L, the etching time is 30 min, recorded as time 3, the water bath temperature is 40° C., recorded as temperature 3, filtering and washing to neutrality, and drying in an oven at 120° C. for 6 h to obtain a fifth catalyst precursor;

[0097] 8) Under the temperature condition of 800° C., recorded as temperature 4, a mixed gas of CO2 with a flow rate of 30 mL / min and N2 with a flow rate of 170 mL / min was introduced into the fifth catalyst precursor, and a third calcination treatment was performed for 10 min, recorded as time 4, to obtain a catalyst;

[0098] 9) Fixing the prepared catalyst in a fluidized bed reactor, reacting silicon tetrachloride with silicon powder at 480° C. and 3 MPa in a hydrogen atmosphere to obtain trichlorosilane product, taking samples for analysis and calculating the conversion rate at 24 h, 48 h, and 72 h of reaction;

[0099] 10) The catalyst was recovered and regenerated after participating in the cold hydrogenation reaction for 72 hours. At a temperature of 800°C, a mixture of CO2 at a flow rate of 30 mL / min and N2 at a flow rate of 170 mL / min was introduced into the catalyst for activation for 5 minutes. The catalyst was then placed in a fixed bed reactor and purged with nitrogen at room temperature and pressure for 1 hour at a flow rate of 50 mL / min. A mixture of hydrogen and nitrogen was then introduced, the temperature was set to 300°C, the flow rate was 50 mL / min, and the catalyst was reduced for 2 hours to obtain a recovered catalyst.

[0100] Example 2

[0101] The preparation method of trichlorosilane in Example 2 is basically the same as that in Example 1, except that the pressure in step 2) is 101 KPa, and the pyrolytic carbon is used as the catalyst carrier without subsequent activation treatment. Specific parameters are shown in Table 1.

[0102] Example 3

[0103] The preparation method of trichlorosilane in Example 3 is basically the same as that in Example 1, except that the pressure in step 2) is 101 KPa. Specific parameters are shown in Table 1.

[0104] Example 4

[0105] The preparation method of trichlorosilane in Example 4 is basically the same as that in Example 1, except that pyrolytic carbon is used as a catalyst carrier and no subsequent activation treatment is performed. Specific parameters are shown in Table 1.

[0106] Example 5

[0107] The preparation method of trichlorosilane in Example 5 is basically the same as that in Example 1, except that step 2) is not performed, and silicon dioxide is used as a catalyst carrier. Specific parameters are shown in Table 1.

[0108] Example 6-25

[0109] The preparation methods of trichlorosilane in Examples 6-25 and Example 1 are basically the same, except that one or more items in the preparation method are changed. Specific parameters are shown in Table 1.

[0110] Comparative Example 1

[0111] The preparation methods of trichlorosilane in Comparative Example 1 and Example 1 are basically the same, except that cuprous chloride is used as a catalyst to participate in the cold hydrogenation reaction. Specific parameters are shown in Table 1.

[0112] Comparative Example 2

[0113] The preparation method of trichlorosilane in Comparative Example 2 is substantially the same as that in Example 1, except that step 5 is not performed. Specific parameters are shown in Table 1.

[0114] Comparative Example 3

[0115] The preparation method of trichlorosilane in Comparative Example 3 is substantially the same as that in Example 1, except that step 6 is not performed. Specific parameters are shown in Table 1.

[0116] Figure 2 The adsorption-desorption curve of the catalyst support prepared in Example 1 of the present invention;

[0117] Figure 3 The pore size distribution diagram of the catalyst carrier prepared in Example 1 of the present invention;

[0118] Figure 4 The adsorption-desorption curve of the catalyst support prepared in Example 2 of the present invention;

[0119] Figure 5 This is a pore size distribution diagram of the catalyst carrier prepared in Example 2 of the present invention;

[0120] Figure 6 The adsorption-desorption curve of the catalyst support prepared in Example 3 of the present invention;

[0121] Figure 7 This is a pore size distribution diagram of the catalyst carrier prepared in Example 3 of the present invention;

[0122] Figure 8 The adsorption-desorption curve of the catalyst support prepared in Example 4 of the present invention;

[0123] Fig. 9 This is the pore size distribution diagram of the catalyst carrier prepared in Example 4 of the present invention.

[0124] from Figure 2-9 It can be seen that Example 1 of the present invention is a porous carbon obtained after negative pressure pyrolysis and activation as a catalyst carrier; Example 2 is a porous carbon obtained after normal pressure pyrolysis and non-activation as a catalyst carrier; Example 3 is a porous carbon obtained after normal pressure pyrolysis and activation as a catalyst carrier; Example 4 is a porous carbon obtained after negative pressure pyrolysis and non-activation as a catalyst carrier. By comparison, it can be seen that the porous carbon prepared after negative pressure pyrolysis and activation in Example 1 has the largest specific surface area and the widest pore size distribution as a catalyst carrier.

[0125] Table 1

[0126]

[0127]

[0128] Table 2 lists the specific surface area, micropore area and micropore volume of the catalyst carriers prepared in Examples 1-4.

[0129] Table 2

[0130] Group <![CDATA[BET specific surface area / m 2 / g]]> <![CDATA[t-Plot micropore area / m 2 / g]]> <![CDATA[t-Plot micropore volume / cm 3 / g]]> Example 1 478.8526 295.0835 0.122618 Example 2 3.4216 0.6020 0.000458 Example 3 194.7572 109.5764 0.046286 Example 4 6.8673 3.1243 0.001316

[0131] From Tables 1-2, it can be seen that, compared with the comparative example, the preparation method of the catalyst provided by the present invention carries out two-layer coating on the catalyst carrier, the silicon dioxide layer is etched by etching treatment, and the thickness of the carbon coating layer is adjusted by the third calcination treatment, so that the catalyst finally forms a hollow structure, so that the catalyst has higher stability and better dispersion of active components, thereby improving the conversion rate of the cold hydrogenation reaction.

[0132] From the comparison between Example 1 and Comparative Examples 1-3, it can be seen that the hollow porous core-shell structure catalyst provided by the present invention has stable catalytic performance. Even if the catalyst is worn in the fluidized bed, the SiO2 porous shell can protect the catalyst, and the active center embedded in the carbon shell can react for a long time without falling off. The hollow structure provides a larger specific surface area, which is conducive to the adsorption and desorption of substances during the reaction process. The hollow porous structure catalyst has high activity in catalytic conversion of silicon tetrachloride and a long service life.

[0133] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a catalyst, characterized in that: The following steps are involved: 1) adding a precipitant to a system including a catalyst support and a metal source to obtain a first catalyst precursor; 2) performing a first calcination treatment and a reduction treatment on the first catalyst precursor in sequence to obtain a second catalyst precursor; 3) performing a carbonization treatment on a system including the second catalyst precursor and a carbon source to obtain a third catalyst precursor; 4) performing a second calcination treatment on the system including the third catalyst precursor and the silicon source to obtain a fourth catalyst precursor; 5) subjecting the fourth catalyst precursor to an etching treatment at 20-80° C. for 0.5-2 h to obtain a fifth catalyst precursor; 6) subjecting the fifth catalyst precursor to a third calcination treatment at 650-1000° C. for 0.1-2 h to obtain the catalyst.

2. The preparation method according to claim 1, characterized in that: The catalyst carrier is porous carbon, which is obtained by subjecting a carbon source to pyrolysis treatment at a pressure of 0.6-1 KPa and then subjecting it to pore expansion treatment.

3. The preparation method according to claim 1 or 2, characterized in that: The carbonization treatment comprises the following steps: introducing a carbon source into the second catalyst precursor at a temperature of 600-1000° C. for 0.1-2 h, maintaining a mass space velocity of 0.01-10 h -1 , maintain for 0.5-1h after the addition.

4. The preparation method according to any one of claims 1 to 3, characterized in that The temperature of the second calcination treatment is 200-500° C., and the time is 1-10 hours.

5. The preparation method according to any one of claims 1 to 4, characterized in that: After adding the precipitant, the pH value of the system is adjusted to 8-12.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The temperature of the reduction treatment is 200-400° C., and the time is 1-5 hours.

7. The preparation method according to any one of claims 1 to 6, characterized in that: Before performing the first calcination treatment on the first catalyst precursor, the method further includes: performing an aging treatment on the first catalyst precursor at 40-80° C. for 1-3 hours.

8. A catalyst, characterized in that Prepared according to the preparation method according to any one of claims 1 to 7.

9. A method for preparing trichlorosilane, characterized in that: The silicon tetrachloride is obtained by catalyzing the catalyst described in claim 8.

10. The method for preparing trichlorosilane according to claim 9, characterized in that: The preparation method comprises the following steps: at a temperature of 300-500° C. and a pressure of 2.5-4 MPa, hydrogen, silicon tetrachloride and silicon powder are introduced into a fluidized bed reactor fixed with the catalyst to carry out gas-solid contact reaction to obtain the trichlorosilane.