Ionic liquid modified solid acid catalyst for preparing isosorbide through sorbitol dehydration as well as preparation method and application of ionic liquid modified solid acid catalyst
By using a solid acid catalyst modified with an ionic liquid, the problems of severe side reactions and low selectivity in the dehydration of sorbitol to isosorbide were solved, and high yield and high selectivity of isosorbide preparation were achieved. The catalyst is reusable and has good stability.
Patent Information
- Application Number
- CN202411112431.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Existing catalysts exhibit severe side reactions and low selectivity in the dehydration of sorbitol to isosorbide, and their stability and separation are difficult, resulting in low isosorbide yield.
Solid acid catalysts modified with ionic liquids are modified by grafting ionic liquids onto solid acid catalysts. This process combines imidazole ionic liquids with solid acids such as niobium oxide, tantalum oxide, and niobium phosphate to form specific binding sites, which are then used for the dehydration reaction of sorbitol.
It improves the yield and selectivity of isosorbide, the catalyst is reusable, reduces costs and pollution, and the catalyst surface has carbon deposition, which improves long-term stability.
Smart Images

Figure BDA0004992631100000051 
Figure BDA0004992631100000061 
Figure BDA0004992631100000062
Abstract
Description
Technical Field
[0001] The invention belongs to the fields of catalytic chemistry and chemical engineering, and particularly relates to an ionic liquid-modified solid acid catalyst for preparing isosorbide by dehydrating sorbitol, and a preparation method and application thereof. Background Art
[0002] Isosorbide is the only saccharide diol that has been industrially produced and is widely used in the fields of medicine, liquid crystal materials, plasticizers, polymers, etc. The difficulty of the preparation process of isosorbide is mainly due to the violent side reactions in the dehydration process and the low selectivity, and the catalyst is the key to the reaction. In industry, the reaction is usually carried out under the action of a strong acid catalyst, including a homogeneous catalyst and a heterogeneous catalyst. However, the homogeneous catalyst is highly corrosive and difficult to separate from the product, and the heterogeneous catalyst has a low catalytic activity and poor stability. These problems make it impossible to optimize the production of isosorbide.
[0003] Solid acid has the advantages of mild reaction conditions, easy product separation, non-corrosiveness, and reusability. Patent CN114671883A discloses a method for preparing isosorbide by dehydration of sorbitol catalyzed by niobium-based solid acid, and the yield of isosorbide is as high as 76%. Patent CN110483678A discloses a series of F-modified polymer-based solid acid catalysts prepared by hydrothermal synthesis, with an isosorbide yield of more than 80%. In order to promote the efficient dehydration of sorbitol to prepare isosorbide, the development of efficient, highly selective, highly stable, and low-cost catalysts and their recycling methods will be the focus of future research.
[0004] The structure of ionic liquids is adjustable, and they can improve the microenvironment of the catalytic active center, provide more acid centers, and realize the controllable preparation of the acid sites of the catalyst. The development of ionic liquid-modified solid acid catalysts provides a new idea for the future development of catalysts. The present invention aims at the problems of violent side reactions and poor selectivity in the preparation process of isosorbide, and discloses a method for catalyzing the preparation of isosorbide from sorbitol using an ionic liquid-modified solid acid catalyst. The catalyst has excellent catalytic activity and easy recovery performance, and has a high catalytic efficiency for the dehydration of sorbitol to produce isosorbide. Summary of the invention
[0005] In view of the problems and shortcomings in the prior art, the object of the present invention is to provide an ionic liquid-modified solid acid catalyst for dehydration of sorbitol to prepare isosorbide, and a preparation method and application thereof.
[0006] Based on the above purpose, the present invention adopts the following technical solution:
[0007] The first aspect of the present invention provides an ionic liquid-modified solid acid catalyst for dehydration of sorbitol to prepare isosorbide, wherein the catalyst is modified by an ionic liquid grafting modification method on a solid acid catalyst; wherein the ionic liquid is any one of imidazoles, pyridines, quaternary ammoniums, quaternary phosphoniums, pyrrolidines, piperidines or functionalized ionic liquids; and the solid acid is any one of niobium oxide, tantalum oxide, niobium phosphate, tantalum phosphate, Al2O3, and Al2O3-SiO2.
[0008] Preferably, the ionic liquid is an imidazolium ionic liquid.
[0009] More preferably, the imidazolium ionic liquid is 1-butyl-3-methylimidazolium chloride.
[0010] Preferably, the solid acid catalyst is niobium oxide (Nb2O5).
[0011] According to the ionic liquid modified solid acid catalyst, preferably, the amount of the ionic liquid is 0.1 wt% to 10 wt% of the mass of the solid acid catalyst.
[0012] The second aspect of the present invention provides a method for preparing the ionic liquid-modified solid acid catalyst described in the first aspect, comprising the following steps:
[0013] (1) adding the ionic liquid into a solvent and stirring to dissolve the ionic liquid to obtain a solution with a concentration of 0.01 to 10 mol / L;
[0014] (2) adding a solid acid catalyst to the solution obtained in step (1), stirring and reacting, and filtering after the reaction to obtain a product;
[0015] (3) adding an acid solution to the product obtained in step (2) for acidification, and removing the solvent to obtain the ionic liquid-modified solid acid catalyst.
[0016] According to the preparation method, preferably, the reaction temperature in step (2) is 20 to 80° C., and the reaction time is 1 to 4 hours.
[0017] According to the preparation method, preferably, the acid solution in step (3) is an inorganic acid solution.
[0018] More preferably, the inorganic acid is any one of sulfuric acid, phosphoric acid, hydrochloric acid and nitric acid.
[0019] More preferably, the inorganic acid is sulfuric acid or phosphoric acid.
[0020] The third aspect of the present invention provides the use of the ionic liquid-modified solid acid catalyst described in the first aspect in the dehydration of sorbitol to prepare isosorbide. The specific operation steps of using the ionic liquid-modified solid acid catalyst in the dehydration of sorbitol to prepare isosorbide are: after the sorbitol solution is dehydrated under high temperature and negative pressure or the solid sorbitol is heated to melt, the ionic liquid-modified solid acid catalyst is added to the sorbitol to carry out a dehydration reaction to prepare isosorbide.
[0021] According to the application, preferably, the amount of the ionic liquid modified solid acid catalyst is 0.1wt% to 20wt% of the mass of sorbitol; the dehydration reaction temperature is 130°C to 200°C; the dehydration reaction pressure is from atmospheric pressure to -0.1MPa; and the reaction time is 1h to 6h.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The method of the present invention adopts ionic liquid as a modifier, prepares a series of solid acid catalysts, takes sorbitol as a raw material, directly prepares isosorbide by dehydration reaction without solvent and under vacuum conditions, has the advantages of high isosorbide yield, good selectivity, simple operation and low pollution, and the isosorbide yield can reach 96%. Among them, the adopted modifier contains various types of functional groups, can form specific binding sites with reactant and intermediate molecules, and is more conducive to the diffusion and mass transfer of reactants and products on the catalyst surface.
[0024] In the method provided by the present invention, the amount of ionic liquid added is 0.1wt%-10wt% of the mass of the catalyst, the amount of addition is small, and the catalyst will not decompose during the reaction process, and the catalyst can be simply reused. The amount of catalyst used is 0.1wt%-20wt% of the mass of solid sorbitol. Compared with the existing preparation method, the amount of catalyst used is greatly reduced, saving costs.
[0025] The catalyst used in the present invention is an ionic liquid modified solid acid catalyst. The ionic liquid and the solid acid each have good catalytic performance for the sorbitol dehydration reaction. After the two are combined and modified, it is more conducive to the diffusion and mass transfer of reactants and products. The combination of the two can effectively avoid carbon accumulation on the surface of the solid acid catalyst and improve the long-term stability of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the pyridine infrared spectrum of the ionic liquid-modified niobium oxide solid acid prepared in Example 1 of the present invention;
[0027] Figure 2 The pyridine infrared spectrum of the ionic liquid-modified tantalum oxide solid acid prepared in Example 2 of the present invention;
[0028] Figure 3This is the pyridine infrared spectrum of the ionic liquid-modified niobium phosphate solid acid prepared in Example 3 of the present invention;
[0029] Figure 4 This is the pyridine infrared spectrum of the ionic liquid modified tantalum phosphate solid acid prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail by way of embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0031] 1. Preparation of ionic liquid modified solid acid catalyst
[0032] Example 1
[0033] This embodiment provides an ionic liquid-modified solid acid catalyst for dehydration of sorbitol to prepare isosorbide, wherein the solid acid catalyst is modified by an ionic liquid grafting modification method; wherein the ionic liquid is 1-butyl-3-methylimidazolium chloride; the solid acid is niobium oxide; and the amount of 1-butyl-3-methylimidazolium chloride used is 0.5wt% of the mass of niobium oxide.
[0034] The preparation method of the ionic liquid modified solid acid catalyst comprises the following steps: (1) adding 1-butyl-3-methylimidazolium chloride into a solvent and stirring and dissolving the mixture to obtain a solution with a concentration of 0.5 mol / L;
[0035] (2) adding 3 g of niobium oxide to 30 mL of the solution obtained in step (1), stirring and reacting at 60° C. for 2 h, and filtering to obtain the product after the reaction is completed;
[0036] (3) adding sulfuric acid to the product obtained in step (2) for acidification, and removing the solvent to obtain an ionic liquid-modified niobium oxide catalyst.
[0037] Example 2
[0038] This embodiment provides an ionic liquid-modified solid acid catalyst for dehydrating sorbitol to prepare isosorbide, wherein the solid acid catalyst is modified by an ionic liquid grafting modification method; wherein the ionic liquid is 1-butyl-3-methylimidazolium chloride; the solid acid is tantalum oxide; and the amount of 1-butyl-3-methylimidazolium chloride used is 0.5wt% of the mass of tantalum oxide.
[0039] The preparation method of the ionic liquid modified solid acid catalyst comprises the following steps: (1) adding 1-butyl-3-methylimidazolium chloride into a solvent and stirring and dissolving the mixture to obtain a solution with a concentration of 0.5 mol / L;
[0040] (2) adding 3 g of tantalum oxide to 30 mL of the solution obtained in step (1), stirring and reacting at 60° C. for 2 h, and filtering to obtain the product after the reaction is completed;
[0041] (3) adding sulfuric acid to the product obtained in step (2) for acidification, and removing the solvent to obtain an ionic liquid-modified tantalum oxide solid acid catalyst.
[0042] Example 3
[0043] This embodiment provides an ionic liquid-modified solid acid catalyst for dehydrating sorbitol to prepare isosorbide, wherein the solid acid catalyst is modified by an ionic liquid grafting modification method; wherein the ionic liquid is 1-butyl-3-methylimidazolium chloride; the solid acid is niobium phosphate, and the amount of 1-butyl-3-methylimidazolium chloride is 0.5wt% of the mass of the niobium phosphate.
[0044] The preparation method of the ionic liquid modified solid acid catalyst comprises the following steps: (1) adding 1-butyl-3-methylimidazolium chloride into a solvent and stirring and dissolving the mixture to obtain a solution with a concentration of 0.5 mol / L;
[0045] (2) adding 3 g of niobium phosphate to 30 mL of the solution obtained in step (1), stirring and reacting at 60° C. for 2 h, and filtering to obtain the product after the reaction is completed;
[0046] (3) adding sulfuric acid to the product obtained in step (2) for acidification, and removing the solvent to obtain an ionic liquid-modified niobium phosphate solid acid catalyst.
[0047] Example 4
[0048] This embodiment provides an ionic liquid-modified solid acid catalyst for dehydrating sorbitol to prepare isosorbide, wherein the solid acid catalyst is modified by an ionic liquid grafting modification method; wherein the ionic liquid is 1-butyl-3-methylimidazolium chloride; the solid acid is tantalum phosphate, and the amount of 1-butyl-3-methylimidazolium chloride is 0.5wt% of the mass of tantalum phosphate
[0049] The preparation method of the ionic liquid modified solid acid catalyst comprises the following steps: (1) adding 1-butyl-3-methylimidazolium chloride into a solvent and stirring and dissolving the mixture to obtain a solution with a concentration of 0.5 mol / L;
[0050] (2) adding 3 g of tantalum phosphate to 30 mL of the solution obtained in step (1), stirring and reacting at 60° C. for 2 h, and filtering to obtain the product after the reaction is completed;
[0051] (3) adding sulfuric acid to the product obtained in step (2) for acidification, and removing the solvent to obtain an ionic liquid-modified tantalum phosphate solid acid catalyst.
[0052] Example 5
[0053] The contents of an ionic liquid-modified solid acid catalyst for dehydrating sorbitol to prepare isosorbide are substantially the same as those of Example 1, except that phosphoric acid is used for acidification.
[0054] Example 6
[0055] The contents of an ionic liquid-modified solid acid catalyst for dehydrating sorbitol to prepare isosorbide are substantially the same as those of Example 2, except that phosphoric acid is used for acidification.
[0056] Example 7
[0057] The contents of an ionic liquid-modified solid acid catalyst for dehydrating sorbitol to prepare isosorbide are substantially the same as those of Example 3, except that phosphoric acid is used for acidification.
[0058] Example 8
[0059] The contents of an ionic liquid-modified solid acid catalyst for dehydrating sorbitol to prepare isosorbide are substantially the same as those of Example 4, except that phosphoric acid is used for acidification.
[0060] Comparative Example 1
[0061] The content of a catalyst for dehydrating sorbitol to prepare isosorbide is substantially the same as that of Example 1, except that no niobium oxide solid acid catalyst is added.
[0062] Comparative Example 2
[0063] The content of a catalyst for dehydrating sorbitol to prepare isosorbide is substantially the same as that of Example 1, except that no 1-butyl-3-methylimidazolium chloride is added.
[0064] Comparative Example 3
[0065] The content of a catalyst for dehydrating sorbitol to prepare isosorbide is substantially the same as that of Example 2, except that no 1-butyl-3-methylimidazolium chloride is added.
[0066] Comparative Example 4
[0067] The content of a catalyst for dehydrating sorbitol to prepare isosorbide is substantially the same as that of Example 3, except that no 1-butyl-3-methylimidazolium chloride is added.
[0068] The ionic liquid modified solid acid catalysts prepared in Examples 1 to 4 were subjected to pyridine infrared testing, and the results are shown in Figures 1 to 4 As shown by Figures 1 to 4It can be found that the characteristic vibration peaks of pyridine adsorbed on Lewis acid sites are detected at 1448cm-1, 1575cm-1 and 1608cm-1, among which 1448cm-1 and 1608cm-1 are strong Lewis acid sites; 1540cm-1 and 1635cm-1 are detected for pyridine adsorbed on The characteristic vibration peak of the acid site is at 1490cm-1, which is Lewis acid and The overlapping characteristic vibration peaks of the acid. It can be seen that there are more Lewis acid sites in the catalyst than Acid sites. Even after vacuum desorption at the reaction temperature (200°C) for 25 minutes, the Lewis acid sites of the catalyst are sufficiently stable. The B / L values of different catalysts under pyridine desorption conditions at 200°C are calculated and shown in Table 1.
[0069] Table 1 Acid properties of [BMIM] modified solid acid catalysts
[0070]
[0071]
[0072] Note: -1 means sulfuric acid acidification, -2 means phosphoric acid acidification.
[0073] As shown in Table 1, the acid characterization results show that sulfuric acid modification can significantly increase the total acid content of the catalyst, and the B acid ratio is higher, indicating that the ionic liquid modification and acid modification mainly affect the B acid properties of the catalyst. For different solid acids, the total acid content is significantly different from BAS / LAS, and is higher than that of the unmodified catalyst, which fully illustrates the effectiveness of ionic liquid modification. The ionic liquid used in the present invention is liquid, and its acid properties cannot be quantitatively or qualitatively evaluated by acid characterization. However, the total acid content of the catalyst without ionic liquid modification is significantly reduced.
[0074] 2. Preparation of Isosorbide by Dehydration of Sorbitol
[0075] 1. Experiment on the catalytic preparation of isosorbide using solid sorbitol as raw material
[0076] The catalysts prepared in Examples 1 to 8 and Comparative Examples 1 to 4 were used to dehydrate solid sorbitol to prepare isosorbide. The specific operation steps were as follows: 30 g of sorbitol was heated in a reactor until it was melted, 2 g of the catalyst prepared in Examples 1 to 8 or Comparative Examples 1 to 4 was added thereto, and after reacting at 5 KPa and 170° C. for 5 h, a sample was taken for high performance liquid chromatography analysis. The results are shown in Table 2.
[0077] Table 2 Chromatographic analysis results
[0078]
[0079] Note: -1 means sulfuric acid acidification, -2 means phosphoric acid acidification.
[0080] As can be seen from Table 2, when [BMIM] / Nb2O5 is used as the catalyst, the catalytic effect is the best, sorbitol can be completely converted, the yield of isosorbide is 96%, and the by-product is mainly 1,4-anhydrosorbitol. The yield of isosorbide in other embodiments of sulfuric acid acidification is higher than 80%, and at the same time, the content of 1,4-anhydrosorbitol is slightly higher than that of niobium oxide system. However, the performance of the solid acid catalyst acidified with phosphoric acid is slightly poor, which may be related to the relatively low total acid content on the catalyst surface. Compared with the comparative example, the performance of the sulfuric acid acidified solid acid catalyst without ionic liquid modification is significantly reduced, indicating that ionic liquid modification can improve the catalyst activity.
[0081] 2. Experiment on the catalytic preparation of isosorbide using sorbitol solution as raw material
[0082] The catalyst prepared by using Examples 1 to 8 and Comparative Examples 1 to 4 is used to dehydrate 37wt% sorbitol solution to prepare isosorbide. The specific operation steps are: add the sorbitol solution to the reactor, heat it to 110°C, turn on the water pump to evacuate, the negative pressure is -0.9MPa, add the catalyst after fully removing water, and then react. Specifically, add 100g, 37wt% sorbitol solution to react, 110°C, -0.9MPa after removing water for 2 hours, add 5g of the catalyst prepared by Examples 1 to 8 or Comparative Examples 1 to 4, react at 170°C for 5h, and take samples for high performance liquid chromatography analysis. The results are shown in Table 3.
[0083] Table 3 Chromatographic analysis results
[0084]
[0085] Note: -1 means sulfuric acid acidification, -2 means phosphoric acid acidification.
[0086] With sorbitol solution as the reactant, the yield of isosorbide decreased by about 10%, and the yield of sulfuric acid-oxidized niobium oxide modified by ionic liquid decreased to 83%, which may be due to the fact that excess water inhibited the dehydration reaction. By comparing Example 1 with Comparative Example 2, it can still be found that ionic liquid modification helps to improve the product yield.
[0087] 3. Repeatability Experiment
[0088] The catalyst prepared in Example 1 was recovered and the experiment was repeated 5 times, and samples were taken for high performance liquid chromatography analysis. The results are shown in Table 4. The catalyst was directly reused after filtering and washing, and still showed good catalytic performance. The yield of isosorbide was still 91.8% after 5 repetitions, and the yield of 1,4-anhydrosorbitol was slightly increased.
[0089] Table 4 Effect of cycle number on the dehydration of sorbitol to prepare isosorbide
[0090]
Claims
1. An ionic liquid-modified solid acid catalyst for dehydrating sorbitol to isosorbide, characterized in that: The solid acid catalyst is modified by an ionic liquid grafting modification method; wherein the ionic liquid is any one of imidazole, pyridine, quaternary ammonium, quaternary phosphonium, pyrrolidine, piperidine or functionalized ionic liquid; and the solid acid is any one of niobium oxide, tantalum oxide, niobium phosphate, tantalum phosphate, Al2O3, and Al2O3-SiO2.
2. The ionic liquid-modified solid acid catalyst according to claim 1, characterized in that The amount of the ionic liquid used is 0.1 wt% to 10 wt% of the mass of the solid acid catalyst.
3. The method for preparing the ionic liquid-modified solid acid catalyst according to claim 1 or 2, characterized in that: The steps include: (1) adding the ionic liquid into the solvent and stirring to dissolve it to obtain a solution with a concentration of 0.01 to 10 mol / L; (2) adding a solid acid catalyst to the solution obtained in step (1), stirring to carry out a reaction, and filtering to obtain a product after the reaction is completed; (3) Adding an acid solution to the product obtained in step (2) for acidification, and removing the solvent to obtain the ionic liquid-modified solid acid catalyst.
4. The preparation method according to claim 3, characterized in that: The reaction temperature in step (2) is 20 to 80° C., and the reaction time is 1 to 4 hours.
5. The preparation method according to claim 3, characterized in that: The acid solution in step (3) is an inorganic acid solution.
6. The preparation method according to claim 5, characterized in that: The inorganic acid is any one of sulfuric acid, phosphoric acid, hydrochloric acid and nitric acid.
7. Use of the ionic liquid-modified solid acid catalyst according to claim 1 or 2 in the dehydration of sorbitol to produce isosorbide.
8. The use according to claim 7, characterized in that: The specific operation steps are: after the sorbitol solution is dehydrated at high temperature and negative pressure or the solid sorbitol is heated to be melted, a solid acid catalyst modified by an ionic liquid is added to the sorbitol to carry out a dehydration reaction to prepare isosorbide.
9. The use according to claim 8, characterized in that: The amount of the ionic liquid modified solid acid catalyst is 0.1wt% to 20wt% of the mass of sorbitol; the dehydration reaction temperature is 130°C to 200°C; the dehydration reaction pressure is from normal pressure to -0.1MPa; and the reaction time is 1h to 6h.
Citation Information
Patent Citations
Immobilized ionic liquid solid acid catalyst and preparation method thereof
CN104525252A
Method of preparing isosorbide by continuous reaction of sorbitol
CN110372716A
Preparation method of isosorbide
CN111253413A
Pyridine polymerized ionic liquid solid acid catalyst, and preparation method and application thereof
CN113856752A
Method for preparing isosorbide by catalyzing dehydration of sorbitol through polymeric ionic liquid
CN115010718A