Collector-free flotation separation method for copper sulfide ore under natural acid-base condition
By using titanium sulfide reagent as an inhibitor and collector under natural acid and alkali conditions, the problems of low copper yield and associated precious metal loss in copper-sulfur flotation separation are solved, and efficient green recovery of copper-sulfur resources is achieved, reducing the Cost and reduce environmental pollution.
Patent Information
- Application Number
- CN202411436254.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-15
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art has problems of low copper yield, associated precious metal loss, high cost and environmental pollution in copper-sulfur flotation separation. Especially when using lime and activators under high alkali conditions, it will lead to calcium blockage in pipeline junction and equipment corrosion.
Using titanium reagent as an inhibitor and collector under natural acid and alkali conditions, the separation effect between chalcopyrite and pyrite is significantly improved through chelation, avoiding the use of lime and activators, and achieving copper-sulfur separation.
It significantly improves the copper-sulphur separation effect, reduces water pollution and pipeline calcium blockage, reduces the cost of medicines, and realizes efficient green recycling of copper-sulphur resources, which has significant economic benefits.
Smart Images

Figure CN119016206A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a collector-free flotation separation method for copper sulfide ore under natural acid-base conditions, belonging to the technical field of mineral separation. Background Art
[0002] Copper has become an indispensable raw material in the industrial field due to its excellent ductility, electrical conductivity, thermal conductivity and corrosion resistance. Copper is widely used in many industries such as electrical, national defense, light industry, batteries, machinery manufacturing, etc., and is an important basic material supporting the development of the national economy.
[0003] Chalcopyrite is the main source of copper metal extraction and is often associated with pyrite. Flotation is the key technology for separating and recovering the two. Since the natural floatability of the two is similar and the collectors used in the flotation process lack selectivity, it is difficult to separate the two.
[0004] At present, the industry mostly uses lime as a pyrite inhibitor, and uses advanced xanthate (such as butyl xanthate and amyl xanthate) to float chalcopyrite under high alkaline conditions to achieve copper and sulfur flotation separation. However, this method not only has problems such as low copper yield and large loss of associated precious metals, but also has high costs for advanced xanthate, which is often accompanied by pungent odors and has adverse effects on the environment. In addition, after adding lime high-alkali inhibition, not only does it need to add a large amount of activator for subsequent sulfur selection operations, but it is also easy to cause problems such as pipeline calcium blockage, equipment corrosion, and water pollution. Summary of the invention
[0005] In order to solve the problems existing in the flotation separation of chalcopyrite and pyrite, the present invention provides a flotation separation method of copper sulfide ore without a collector under natural acid-base conditions, which can realize copper-sulfur separation under natural acid-base conditions without adding lime and activator, and can realize green and low-cost recovery of pyrite.
[0006] The specific steps are as follows:
[0007] (1) Under natural acid and alkali conditions, the copper sulfide ore is ground, and a dispersant, an inhibitor, and a frother are sequentially added to the slurry to perform a roughing operation. After the roughing operation, an inhibitor and a frother are added to perform two sweeping operations. After the sweeping operation, two concentration operations are performed to obtain copper concentrate and copper tailings, wherein the intermediate ore products are sequentially returned;
[0008] The inhibitor is an iron-titanium reagent, and the amount added in the first rough selection is 500-700 g / t, and the amount added in the two sweep selections is 150-250 g / t respectively.
[0009] (2) adding a collector and a frother to the copper tailings obtained in step (1) in sequence, and performing a roughing selection. After the roughing selection is completed, adding a collector, and performing two scavenging selections; after the scavenging selections are completed, two concentrating selections are performed to obtain sulfur concentrate and tailings, wherein the intermediate ore products are returned in sequence.
[0010] Preferably, the dispersant in step (1) is water glass, and the amount added in the first rough selection is 2000-3000 g / t. The foaming agent is No. 2 oil, and the amount added in the first rough selection is 20 g / t, and the amount added in the two sweep selections is 10 g / t respectively.
[0011] Preferably, the copper roughing operation in step (1) lasts for 6 minutes, each scavenging operation lasts for 4 minutes, and each concentrating operation lasts for 5 minutes.
[0012] Preferably, the sulfur collector in step (2) is butyl xanthate, the amount added in the first rough selection is 150-200 g / t, and the amount added in the two sweep selections is 80-100 g / t respectively; the foaming agent is No. 2 oil, the amount added in the first rough selection is 10-15 g / t.
[0013] Preferably, in step (2), the duration of the sulfur roughing operation is 6 minutes, the duration of each scavenging operation is 4 minutes, and the duration of each cleaning operation is 5 minutes.
[0014] Principle of the invention: The inhibitor ferrotitanium reagent used in the invention is a chelating inhibitor, which contains hydrophilic sulfonic acid groups in its molecular structure, and can be selectively adsorbed on the surface of pyrite through chelation, which can significantly increase the hydrophilicity of the pyrite surface; in addition, the ferrotitanium reagent can react with the hydroxide formed by oxidation on the surface of chalcopyrite to generate a water-soluble chelate, which removes the hydrophilic species and has the effect of improving the floatability of chalcopyrite, thereby achieving the separation of chalcopyrite and pyrite. The selective inhibition characteristics of the ferrotitanium reagent give it a significant application advantage in the flotation process of copper sulfide ores.
[0015] Beneficial effects of the present invention
[0016] (1) The pyrite inhibitor ilmenite reagent provided by the present invention has strong selectivity and can significantly improve the separation effect of chalcopyrite and pyrite in copper sulfide ore under natural acid-base conditions.
[0017] (2) Compared with the traditional method of using a large amount of lime for high alkali suppression, the present invention does not use lime to adjust the pH of the slurry, but realizes copper-sulfur separation under natural acid-base conditions, which can reduce water pollution and pipeline calcium blockage.
[0018] (3) The method of the present invention does not add a collector in the copper separation operation, and does not add an activator in the sulfur separation operation. Compared with the traditional flotation separation method of copper sulfide ore, it greatly saves the cost of reagents.
[0019] (4) The method of the present invention uses fewer types of flotation agents, and flotation control is simpler, thereby achieving efficient and green recovery of copper and sulfur resources and having significant economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is the flotation flow chart of the present invention.
[0021] Figure 2 This is the flotation flow chart of Comparative Example 1. DETAILED DESCRIPTION
[0022] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0023] The minerals used in the following examples are copper sulfide ores from a copper mine in Yunnan Province, with a copper grade of 0.6-0.7% and a sulfur grade of 10-11%. The copper-containing minerals are mainly chalcopyrite, accounting for 80-85%; and the pyrite is mainly pyrite.
[0024] Example 1
[0025] This example corresponds to the original ore with a copper grade of 0.60% and a sulfur grade of 10.01%. Titanium-iron reagent is used as a depressant to separate copper and sulfur. The flotation flow chart is as follows: Figure 1 The dosage of the drugs is shown in Table 1.
[0026] Table 1 Example 1 Dosage of medicine
[0027]
[0028] The specific steps are as follows:
[0029] (1) Grind the copper sulfide ore to a fineness of -74 μm, accounting for 75%.
[0030] (2) Under natural acid and alkali conditions, dispersant water glass, inhibitor titanium iron reagent, and foaming agent No. 2 oil are added in sequence for a roughing operation, and the roughing operation time is 6 minutes. After the roughing is completed, the inhibitor titanium iron reagent and foaming agent No. 2 oil are added for two sweeping operations, and the sweeping operation time is 4 minutes each. After the sweeping is completed, two fine selections are carried out, and the fine selection operation time is 5 minutes each, to obtain copper concentrate and copper tailings, during which the ore products are returned in sequence.
[0031] (3) In the copper tailings obtained in step (2), butyl xanthate collector and No. 2 oil frother were added in sequence to carry out a roughing operation for 6 minutes. After the roughing operation, butyl xanthate collector was added to carry out two scavenging operations. The scavenging operation lasted for 4 minutes. After the scavenging operation, two concentration operations were carried out to obtain sulfur concentrate and tailings, wherein the intermediate ore products were returned in sequence. The flotation indicators are shown in Table 2.
[0032] Table 2 Flotation index of Example 1
[0033]
[0034] When the method of the present invention is used to process relatively low-grade raw ore, Example 1 obtains a copper concentrate with a copper grade of 20.11% and a copper recovery rate of 90.16%; and obtains a sulfur concentrate with a sulfur grade of 48.71% and a sulfur recovery rate of 80.78%. The results show that the copper-sulfur separation effect of Example 1 is obvious, and high-quality copper concentrate and sulfur concentrate are produced.
[0035] Example 2
[0036] This example corresponds to the original ore with a copper grade of 0.65% and a sulfur grade of 10.57%. Except for the properties of the mineral raw materials, the specific operation process is the same as that of Example 1, the dosage of the reagent is shown in Table 3, and the flotation index is shown in Table 4.
[0037] Table 3 Example 2 dosage
[0038]
[0039] Table 4 Flotation index of Example 2
[0040]
[0041] From the results in Table 4, it can be seen that under natural acid-base conditions, the use of ferro-titanium reagent as a pyrite inhibitor yielded a copper concentrate with a copper grade of 21.04% and a copper recovery rate of 89.99%, and high-quality concentrate indicators were obtained. The subsequent copper tailings selection process adopted a one-rough, two-fine, and two-sweep process to obtain a sulfur concentrate with a sulfur grade of 49.88% and a sulfur recovery rate of 79.34%, achieving efficient separation of copper and sulfur.
[0042] Example 3
[0043] This example corresponds to the original ore with a copper grade of 0.69% and a sulfur grade of 10.89%. Except for the properties of the mineral raw materials, the specific operation process is the same as that of Example 1, the dosage of the reagent is shown in Table 5, and the flotation index is shown in Table 6.
[0044] Table 5 Example 3 dosage
[0045]
[0046] Table 6 Flotation index of Example 3
[0047]
[0048] When the method of the present invention is used to treat relatively high-grade raw ore, the required amount of dispersant, inhibitor and collector needs to be appropriately increased; Example 3 produces a copper concentrate with a copper grade of 21.63% and a copper recovery rate of 89.97%; a sulfur concentrate with a sulfur grade of 51.25% and a sulfur recovery rate of 79.91%. The flotation indexes of Example 3 are similar to those of Example 1 and Example 2, indicating that the method has strong adaptability in treating this type of copper-sulfur ore and can well achieve copper-sulfur separation.
[0049] Comparative Example 1
[0050] The mineral raw materials are the same as those in Example 1, the process variables are described in the specific implementation mode, and the conditions not described are the same as those in Example 1. Figure 2 The flotation reagent dosage is shown in Table 7.
[0051] Table 7 Comparative Example 1 Medicament dosage
[0052]
[0053] The specific steps are as follows:
[0054] (1) Add lime as an inhibitor during grinding to adjust the pH of the slurry to around 12.
[0055] (2) Collector I isoamyl xanthate and frother No. 2 oil are added to the slurry in sequence for a roughing operation of 6 minutes. After the roughing operation, collector I isoamyl xanthate and frother No. 2 oil are added again for two scavenging operations of 4 minutes each. After the scavenging operation, two concentrating operations are carried out of 5 minutes each to obtain copper concentrate and copper tailings, wherein the intermediate ore products are returned in sequence.
[0056] (3) The copper tailings obtained in step (2) are sequentially added with activator copper sulfate, collector II butyl xanthate, and frother oil for a roughing process, the roughing time is 6 minutes, and after the roughing process, collector II butyl xanthate is added again for two scavenging processes, each scavenging time is 4 minutes, and after the scavenging process, two fine processes are performed, each time for 5 minutes, to obtain sulfur concentrate and tailings, wherein the intermediate ore products are sequentially returned; the flotation indicators are shown in Table 8.
[0057] Table 8 Comparative Implementation Example 1 Flotation Index
[0058]
[0059] As can be seen from Table 8, the copper concentrate with a copper grade of 19.64% and a copper recovery rate of 84.78% was obtained in Comparative Example 1; the sulfur concentrate with a sulfur grade of 45.23% and a sulfur recovery rate of 72.07% was obtained. Compared with Example 1, the flotation indexes of copper concentrate, copper recovery rate of copper concentrate, sulfur grade of sulfur concentrate and sulfur recovery rate of sulfur concentrate were all reduced.
[0060] By comparing Example 1 with Comparative Example 1, it is found that the separation of copper sulfide ore can be achieved by adjusting the pH of the slurry to high alkaline conditions using a large amount of lime, but because lime also has a certain inhibitory effect on chalcopyrite, it will cause the chalcopyrite to be lost in the subsequent sulfur concentrate; at the same time, because the copper selection operation uses a large amount of lime to inhibit pyrite, the sulfur selection operation requires a large amount of activator to activate pyrite, and the activation effect is affected to a certain extent, which leads to a low sulfur recovery rate of the sulfur concentrate. Therefore, the copper and sulfur recovery effect of the method in Comparative Example 1 for treating this type of ore is poor, and the production cost is higher. The inhibitor titanium iron reagent of the present invention does not need to adjust the pH, but realizes the efficient separation of chalcopyrite and pyrite in the copper sulfide ore under natural acid and alkaline conditions, and is a high-quality copper-sulfur separation inhibitor, while ensuring the quality of copper concentrate. In addition, no activator is required in the process flow, which greatly saves the cost of reagents.
[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made on the basis of the present invention should be included in the protection scope of the present invention.
Claims
1. A collector-free flotation separation method for copper sulfide ore under natural acid-base conditions, characterized in that: The specific steps are as follows: (1) grinding the copper sulfide ore, adding a dispersant, an inhibitor, and a frother in the ore pulp in sequence, performing a roughing operation, adding an inhibitor and a frother after the roughing operation, performing two sweeping operations, and performing two concentrating operations after the sweeping operation to obtain a copper concentrate and a copper tailings; The inhibitor is an iron-titanium reagent, and the amount added in the first rough selection is 500-700 g / t, and the amount added in the two sweep selections is 150-250 g / t respectively; (2) adding a collector and a frother to the copper tailings obtained in step (1) in sequence, and performing a roughing selection. After the roughing selection is completed, adding a collector, and performing two scavenging selections; after the scavenging selections are completed, two concentrating selections are performed to obtain sulfur concentrate and tailings, wherein the intermediate ore products are returned in sequence.
2. The method for flotation separation of copper sulfide ore without collector under natural acid-base conditions according to claim 1, characterized in that: The dispersant in step (1) is water glass, and the amount added in the first rough selection is 2000-3000 g / t. The foaming agent is No. 2 oil, and the amount added in the first rough selection is 20 g / t, and the amount added in the two sweep selections is 10 g / t respectively.
3. The method for flotation separation of copper sulfide ore without collector under natural acid-base conditions according to claim 1, characterized in that: The sulfur collector in step (2) is butyl xanthate, and the amount added in the first rough selection is 150-200 g / t, and the amount added in the two sweep selections is 80-100 g / t respectively; the foaming agent is No. 2 oil, and the amount added in the first rough selection is 10-15 g / t.
Citation Information
Patent Citations
Method for acquiring high-quality sulfur concentrates from copper tailings
CN102441492A
Ore dressing method for metal containing secondary copper sulfide ores
CN110292983A
Method for inhibiting flotation of pyrite in minerals
CN115007323A
ARYL ether monosulfonate collectors useful in the flotation of minerals
WO1995003891A1