High-strength flexible anti-electromagnetic interference shielding film and preparation method thereof
Through the blending and grinding of a modified adhesive and a modified alloy and the vulcanization treatment of the organic diaphragm layer, the existing electromagnetic interference-resistant films have been solved in the problem of insufficient performance in moisture and high temperatures, and a high-strength flexible and high-temperature resistance is prepared. Electromagnetic interference shielding film.
Patent Information
- Application Number
- CN202411125023.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
Existing anti-electromagnetic interference films are prone to corrosion when facing humid environments, and their mechanical strength and anti-electromagnetic interference performance are insufficient, especially at high temperatures, which significantly reduce their performance.
The modified adhesive is blended and ground with the modified alloy, and the composite frame layer is formed by vulcanizing the organic separator layer, which enhances the mechanical properties and electromagnetic shielding ability of the film.
It realizes a high-strength and flexible electromagnetic interference-resistant shielding film, with excellent mechanical strength, high temperature resistance and high-efficiency electromagnetic shielding effect.
Smart Images

Figure CN119017809A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of anti-electromagnetic interference film processing, and in particular to a high-strength and flexible anti-electromagnetic interference shielding film and a preparation method thereof. Background Art
[0002] The development of anti-electromagnetic interference films reflects the progress of materials science and electronic engineering. The earliest anti-EMI technology can be traced back to the mid-20th century, when metal films (such as aluminum and copper) were mainly used for shielding. These films were prepared by physical deposition techniques (such as evaporation deposition) for basic electromagnetic interference protection.
[0003] In recent years, with the miniaturization and intelligence of electronic products, anti-EMI films are required to have higher performance and a wider range of applications. Researchers are constantly exploring new functional materials and intelligent coating technologies, such as nanomaterials and multi-layer composite films, to cope with emerging electromagnetic interference problems. At the same time, global standards and specifications for electromagnetic compatibility are constantly updated, promoting the continuous advancement of anti-EMI film technology.
[0004] For example, the prior art CN116442604A discloses a flexible anti-electromagnetic interference film, which specifically includes a first oxide layer, a metal nickel layer is bonded to the bottom of the first oxide layer, a metal copper layer is fixedly bonded to the lower surface of the metal nickel layer, a thin film layer is bonded and fixed to the lower surface of the metal copper layer, a superconducting graphite shielding layer is bonded and fixed to the lower surface of the thin film layer, and a second oxide layer is fixed to the bottom of the superconducting graphite shielding layer. The thin film layer, metal nickel layer, metal copper layer and superconducting graphite shielding layer are arranged, and the metal nickel layer, metal copper layer and superconducting graphite shielding layer are all attached and fixed on the thin film layer. The thin film layer is flexible, so it is based on bending and kneading the thin film layer. Even if the metal copper layer and the metal nickel layer are broken, the entire anti-electromagnetic interference film is not easy to crack. The design of the superconducting graphite shielding layer greatly enhances the anti-interference performance of the anti-electromagnetic interference film, thereby achieving the effect of enhancing the flexibility and anti-electromagnetic interference of the anti-electromagnetic interference film.
[0005] The above content achieves the purpose of anti-electromagnetic interference and flexibility by setting up a large number of hierarchical structures, but the metal hierarchical structure is heavy and costly, and is easily corroded in the face of moisture. The metal hierarchical structure whose surface has not been modified has weak adhesion to the remaining hierarchical structures and is prone to cracking, thereby reducing the performance of the anti-electromagnetic interference film. The film used therein is a polyethylene terephthalate film, which has poor high temperature resistance, while the metal sheet structure and the superconducting graphite shielding layer have strong thermal conductivity, which can easily cause the polyethylene terephthalate film to become brittle at high temperatures, thereby reducing the magnetic properties of the anti-electromagnetic interference film.
[0006] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention
[0007] The purpose of the present invention is to provide a high-strength and flexible anti-electromagnetic interference shielding film and a preparation method thereof, so as to solve the technical problem that the anti-electromagnetic interference performance and mechanical strength of the anti-electromagnetic interference shielding film in the prior art need to be further improved.
[0008] The object of the present invention can be achieved by the following technical solution: A high-strength and flexible anti-electromagnetic interference shielding film comprises an alloy skeleton layer, the outside of which is coated with an organic diaphragm layer;
[0009] The composite skeleton layer is obtained by coating a mixture of a modified adhesive and a modified alloy and curing the mixture on the surface of an organic diaphragm layer, and the organic diaphragm layer is obtained by processing a modified polyamide resin.
[0010] Furthermore, the preparation method of the modified adhesive is as follows: 8-10 parts of amidated polyurethane, 8-10 parts of 4-cyclohexene-1,2-dicarboxylic acid diglycidyl ester, 3-5 parts of vinyl-terminated T-phenyl polysiloxane, 0.3-0.5 parts of azobisisobutyronitrile and 30-40 parts of dimethyl sulfoxide are weighed by weight and added into a reactor, the temperature of the reactor is increased to 50-70°C, the reaction is kept warm for 2-4 hours, and the modified adhesive is obtained by post-treatment.
[0011] The reaction equation for synthesizing the modified adhesive is:
[0012]
[0013] Where:
[0014] R0:
[0015] R2:
[0016] R3:
[0017] The reaction principle of synthesizing the modified adhesive is: under the action of the free radical initiator azobisisobutyronitrile, amidated polyurethane, 4-cyclohexene-1,2-dicarboxylic acid diglycidyl ester and vinyl-terminated T-phenyl polysiloxane undergo free radical polymerization to finally generate a modified adhesive.
[0018] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and distilled under reduced pressure until no liquid is extracted to obtain a modified adhesive.
[0019] Furthermore, the preparation method of the amidated polyurethane is as follows: 20-30 parts of activated polyurethane, 5-10 parts of N,N'-di(2-naphthyl)-p-phenylenediamine, and 75-100 parts of dimethyl sulfoxide are weighed by weight and added into a reaction kettle, stirred at room temperature for 5-10 minutes, the temperature of the reaction kettle is lowered to 0-5°C, 1-2 parts of 1-hydroxybenzotriazole and 1-2 parts of dicyclohexylcarbodiimide are added thereto, the reaction is kept warm for 1-2 hours, and post-processed to obtain the amidated polyurethane.
[0020] The reaction equation for synthesizing amidated polyurethane is:
[0021]
[0022] Where:
[0023] R1:
[0024] The reaction principle for synthesizing amidated polyurethane is as follows: the carboxyl group in the activated polyurethane reacts with carbodiimide to generate an active intermediate, and the amino group and carboxyl group undergo nucleophilic attack to generate a condensation product. Since the addition intermediate of the acid to carbodiimide in the first stage of the reaction is not stable, the addition of acylation catalyst 1-hydroxybenzotriamineazole makes the reaction stable and thorough, and finally the amidated polyurethane is obtained.
[0025] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and distilled under reduced pressure until no liquid is extracted to obtain amidated polyurethane.
[0026] The preparation method of activated polyurethane is as follows: 20-30 parts of hybrid polyurethane, 3-5 parts of maleic anhydride, 75-100 parts of N,N-dimethylformamide and 1-3 parts of triethylamine are weighed and added into a reaction kettle, the temperature of the reaction kettle is increased to 40-60°C, the reaction is kept warm for 2-4 hours, and the activated polyamide resin is obtained by post-treatment.
[0027] The reaction equation for synthesizing activated polyamide resin is:
[0028]
[0029] The reaction principle for synthesizing activated polyamide resin is as follows: under alkaline conditions, the hydrogen ions of the hydroxyl groups on the benzene ring attack the carbonyl carbon atom in 2,3-biphenyl maleic anhydride, and a ring-opening reaction occurs to obtain activated polyamide resin.
[0030] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and the reaction liquid is distilled under reduced pressure until no liquid is extracted to obtain an activated polyamide resin.
[0031] Furthermore, the preparation method of the hybrid polyurethane is as follows: 20-30 parts of modified polyurethane, 5-10 parts of cyclopentanone, 75-100 parts of N,N-dimethylformamide and 1-3 parts of benzene are weighed and added into a reactor, the reactor is heated to 70-90° C., and post-processed to obtain the hybrid polyurethane.
[0032] The reaction equation for synthesizing hybrid polyurethane is:
[0033]
[0034] The reaction principle for synthesizing hybrid polyurethane is as follows: the imine carbon in the modified polyurethane acts as a nucleophilic reagent to attack the carbonyl carbon in the cyclopentanone molecule to form a five-membered ring intermediate formed by a nitrogen anion and a carbonyl carbon. The five-membered ring intermediate undergoes proton transfer or other elimination reactions to eventually form an enone structure to obtain a hybrid polyurethane.
[0035] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and the mixture is distilled under reduced pressure until no liquid is extracted to obtain a hybrid polyurethane.
[0036] Furthermore, the preparation method of the modified polyurethane is as follows: 5-8 parts of 1,4-butene diol, 4-6 parts of 1,6-hexamethylene diisocyanate and 40-50 parts of N,N-dimethylformamide are weighed by weight and added into a reactor, the temperature of the reactor is increased to 70-90°C, the reactor is stirred for 2-4 hours, and the modified polyurethane is obtained by post-treatment.
[0037] The reaction equation for synthesizing modified polyurethane is:
[0038]
[0039] The reaction principle for synthesizing modified polyurethane is as follows: the isocyanate group of 1,6-hexamethylene diisocyanate reacts with the hydroxyl group of 1,4-butenediol to form a polymer connected by carbamate. During this process, the hydroxyl oxygen atom acts as a nucleophilic reagent to attack the isocyanate carbon atom to generate carbamate; the isocyanate group in 3,4',5-trihydroxystilbene reacts with the hydroxyl group of 3,3'-dimethyl-4,4'-biphenyl diisocyanate to form a long-chain structure, and finally the modified polyurethane is obtained.
[0040] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and the reaction liquid is distilled under reduced pressure until no liquid is extracted to obtain modified polyurethane.
[0041] Furthermore, the preparation method of the modified alloy comprises the following steps:
[0042] A1. Weigh 20-30 parts of Sendust magnetic powder and 2-3 parts of multilayer graphene by weight, add them into a pulverizer and grind them, and pass them through a 300-500 mesh sieve to obtain alloy powder;
[0043] A2, weighing 10-20 parts of alloy powder, 40-60 parts of deionized water, 0.01-0.02 parts of chromic acid and 0.2-0.4 parts of phosphoric acid by weight, adding them into a reactor and stirring, raising the temperature of the reactor to 80-90° C., stirring until dry powder state, and post-treating to obtain a modified alloy precursor;
[0044] A3. Place the modified alloy precursor in a -2 -10 -3 Into a 300-4000 ton ammonia nitriding furnace, high-purity ammonia is introduced, the gas pressure is maintained at 0.1-0.5 Torr, the temperature is raised to 500-800°C, the reaction is kept at this temperature for 2-3 hours, and the sample chamber is gradually cooled to room temperature to obtain a modified alloy.
[0045] Furthermore, in step A2, post-treatment includes: placing the dry powder in a drying oven at a temperature of 200° C. for vacuum drying for 1-2 hours to obtain a modified alloy precursor.
[0046] Furthermore, the preparation method of the modified polyamide resin is as follows: 20-30 parts of N,N'-dimethyloxamide, 5-10 parts of hexafluorodianhydride, 75-100 parts of dimethyl sulfoxide and 1-3 parts of triethylamine are weighed by weight and added into a reaction kettle, stirred at room temperature for 2-4 hours, and post-treated to obtain the modified polyamide resin.
[0047] The reaction equation for synthesizing modified polyamide resin is:
[0048]
[0049] The reaction principle for synthesizing modified polyamide resin is as follows: the secondary amino group of N-(2-ethoxyphenyl)-N'-(4-ethylphenyl)-oxalamide acts as a nucleophilic reagent to attack the carbonyl carbon atom in the 3,4,9,10-perylenetetracarboxylic anhydride molecule, wherein the nitrogen atom of the secondary amino group carries a lone pair of electrons, which can form a new covalent bond with the carbonyl carbon atom to form an amide acid polymer, thereby finally preparing a modified polyamide resin.
[0050] Furthermore, the post-treatment includes: after the reactor is cooled to room temperature, the reaction liquid is added into a rotary evaporator with a water bath temperature of 80-100° C., and the reaction liquid is distilled under reduced pressure until no liquid is extracted to obtain a modified polyamide resin.
[0051] Furthermore, the method for preparing the organic diaphragm layer comprises the following steps:
[0052] B1. 80-100 parts of modified polyamide resin, 2-3 parts of reinforcing agent, 2-3 parts of antioxidant, 5-8 parts of wetting agent, 1-5 parts of filler and 200-300 parts of dimethyl sulfoxide are weighed and added into a reaction kettle. The temperature of the reaction kettle is raised to 50-60° C. and stirred for 2-3 hours to obtain an organic glue solution.
[0053] B2. Pour the organic glue into an electrospinning machine, set the voltage of the electrospinning machine to 20-25 kV, set the spinning distance to 20-30 cm, control the flow rate to 0.5-1 L / h, and the spinning thickness to 15-20 μm, and post-treat to obtain an organic diaphragm layer.
[0054] Furthermore, in step B1, the reinforcing agent is one or more of polyvinyl pyrrolidone, polypropylene and polyvinyl fluoride, the anti-aging agent is one or more of diacetyl imide, styrene imine, zinc sulfide and diisopropylbenzene peroxide, the wetting agent is one or more of pyrrolidone, sodium alkylbenzene sulfonate and calcium alkylbenzene sulfonate, and the filler is one or two of nano-silica particles and nano-alumina particles; in step B2, post-treatment includes: after spinning is completed, placing the spinning product in a drying oven at a temperature of 80°C and vacuum drying it until the spinning product has a constant weight to obtain an organic diaphragm layer.
[0055] The present invention also provides a method for preparing a high-strength and flexible anti-electromagnetic interference shielding film, comprising the following steps:
[0056] S1. Weigh 8-10 parts of modified binder, 1-2 parts of γ-aminopropyltriethoxysilane and 5-8 parts of modified alloy by weight, add them into a pulverizer and grind them. After passing through a 300-mesh sieve, add them into a reaction kettle and stir them evenly to obtain alloy powder.
[0057] S2, cutting the organic diaphragm layer obtained by the reaction by a CNC cutting machine to obtain two square organic diaphragm layers with a side length of 200 mm;
[0058] S3. Weigh 20-30 parts of alloy powder, 2-3 parts of sodium dodecyl sulfate, 1-2 parts of polyethylene glycol, 20-30 parts of 8-16wt% sodium hydroxide solution and 20-30 parts of N,N-dimethylformamide by weight and add them to the extrusion coating machine pump. Apply the slurry to one side of two square organic diaphragm layers with a side length of 200 mm through the extrusion port in a constant magnetic field of 20-40mT. Put the spin-coated surfaces of the two organic diaphragms tightly together and dry them at room temperature for 20-24h, then put them into a vulcanizer. Set the temperature of the vulcanizer to 180-200℃, the pressure to 5-10MPa, and the time to 3-5min to obtain an anti-electromagnetic interference diaphragm.
[0059] The reaction equation for preparing the anti-electromagnetic interference diaphragm is:
[0060]
[0061] Where:
[0062] R4:
[0063] R5:
[0064] The reaction principle for preparing the anti-electromagnetic interference diaphragm is as follows: on the contact surface between the organic diaphragm layer and the adhesive, the hydroxyl groups of the epoxy group and the polyamic acid group undergo a ring-opening reaction under alkaline conditions, and the modified adhesive is tightly combined with the organic diaphragm layer to obtain the anti-electromagnetic interference diaphragm.
[0065] The present invention has the following beneficial effects:
[0066] 1. In the process of preparing a high-strength and flexible anti-electromagnetic interference shielding film, the present invention first prepares a modified polyurethane, and obtains an adhesive with a complex spatial structure and active functional groups by hybridization, activation, amidation and free radical polymerization, and obtains a modified alloy by mixing iron silicon aluminum magnetic powder with multilayer graphene and then coating it with a phosphorus shell and then nitriding the surface. The surface nitridation after phosphorus shell coating further enhances its anti-electromagnetic interference ability and compatibility with the adhesive. Furthermore, the dispersibility of the modified alloy in the adhesive is further enhanced by blending and grinding the adhesive, silane coupling agent and modified alloy. Finally, an organic diaphragm with high mechanical properties and heat resistance is obtained by copolymerizing N,N'-dimethyloxamide and hexafluorodianhydride. The hydroxyl groups on its surface can undergo a ring-opening reaction with the epoxy groups in the adhesive, further enhancing its bonding ability with the adhesive. At the same time, its internal strong conjugated structure cooperates with the modified alloy to improve the anti-electromagnetic interference ability of the film, and finally an anti-electromagnetic interference shielding film with strong anti-electromagnetic resistance, high flexibility, high temperature resistance and high mechanical properties is prepared.
[0067] 2. In the process of preparing a modified adhesive of the present invention, a modified polyurethane with a long-chain structure is first prepared. The long-chain structure ensures the flexibility of the polyurethane and ensures its flexibility as an adhesive base material; further, in the process of preparing a hybrid polyurethane, the cyclopentanone as a branch reacts with the secondary amino group in the modified polyurethane to form a cyclic structure with double bonds. In the process of hybridization, a large amount of secondary amino groups are consumed, so that the subsequent reaction proceeds in the direction of the positive reaction, and the large amount of double bond structures generated greatly enhance the complexity of the subsequent free radical reaction, making the spatial structure of the formed product more complex, and the cyclic structure also enhances the mechanical strength and heat resistance of the product; further, in the process of preparing an activated polyamide resin, maleic anhydride consumes a large amount of hydroxyl groups in the process of reacting with the hybrid polyurethane, reducing the occurrence of side reactions, so that the reaction proceeds in the expected direction, and while further introducing double bonds into the long-chain structure, carboxyl groups are introduced, thereby improving the product. activity, providing an active basis for subsequent modification; further, in the process of preparing amidated polyurethane through amidation reaction, the spatial complexity of the long-chain structure is improved, and the introduced amide group and benzene ring further improve the heat resistance and mechanical strength of the product. At the same time, due to the highly symmetrical planar structure and π electron cloud of the benzene ring, the benzene ring can effectively absorb and scatter electromagnetic waves, thereby improving the electromagnetic shielding performance of the material, and the conjugated structure of N,N'-di(2-naphthyl)p-phenylenediamine further improves the material's anti-electromagnetic interference ability; finally, a modified adhesive is prepared by copolymerization through double bond free radical polymerization reaction. Due to the further introduction of double bonds into the polyurethane during the hybridization and activation process, the amidated polyurethane has a large number of double bonds, which makes the adhesive have an extremely complex spatial structure. At the same time, the modification of epoxy and silyl groups also makes the adhesive have a certain flexibility while having strong mechanical strength, and finally a modified adhesive with high mechanical properties, high flexibility and high temperature resistance is obtained.
[0068] 3. In the process of preparing a modified alloy, the multilayer graphene in the alloy powder prepared by the present invention improves the conductivity of the material, and the rich hierarchical structure of the multilayer graphene enables part of the magnetic powder to be dispersed on the graphene surface by inlaying and the like, further enhancing its dispersibility and stability, making it more stable when mechanical stress and external structure change; the phosphorus shell alloy powder structure further improves the thermal stability and dispersibility of the alloy powder, reduces the aggregation and agglomeration between the magnetic powders, thereby maintaining the magnetic properties of the magnetic powder stable. During the nitriding process, the phosphorus shell structure forms a stable surface protective layer, providing additional protection during the nitriding process, avoiding direct contact between the magnetic powder and the corrosive substances in the nitriding atmosphere. Furthermore, the phosphorus shell promotes the uniform penetration of the nitriding gas, improves the uniformity and efficiency of the nitriding process, and helps to achieve a higher quality nitriding layer; further, the nitriding treatment improves the magnetic permeability of the magnetic powder, thereby more effectively shielding electromagnetic interference, reducing the impact of interference signals, and reducing magnetic The magnetic loss of the powder is reduced, making it more stable in the electromagnetic field, further improving the anti-electromagnetic interference ability of the magnetic powder, and the nitriding treatment enhances the structural stability of the magnetic powder, reduces the performance fluctuation caused by electromagnetic interference, and the nitriding treatment further improves the compatibility of the modified alloy with the adhesive, and further improves the dispersibility of the modified alloy in the adhesive, and finally obtains a modified alloy with strong anti-electromagnetic interference performance and high temperature resistance. Furthermore, in the process of preparing the organic diaphragm of the present invention, the strong conjugated structure of N, N'-dimethyloxamide in the modified polyamide resin first prepared can cooperate with the modified alloy to enhance the anti-electromagnetic interference ability of the film, a large number of fluorine groups also further enhance the thermal stability of the organic diaphragm, the amide group increases the hydrogen bonding effect between molecules, and enhances the mechanical strength and stability of the organic film, and the carboxyl group inside it also undergoes a ring-opening reaction with the epoxy group in the adhesive to enhance the binding ability of the two, and finally obtains an organic diaphragm with high temperature resistance and high mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0070] Figure 1 It is a schematic diagram of the overall three-dimensional structure of the present invention;
[0071] In the figure: 100, alloy skeleton layer; 200, organic diaphragm layer. DETAILED DESCRIPTION
[0072] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0073] The content of the sendust magnetic powder used in the present invention is 5.4wt% aluminum, 9.6wt% silicon and 85.0% iron, and the minimum particle size is 50μm;
[0074] The multilayer graphene used in the present invention has a transparency greater than 97%, a minimum particle size of 75 μm, a maximum thickness of 10 nm, and a number of layers of 10-15;
[0075] The polyethanol used in the present invention has a relative density of 1.130 and a molecular weight of 3000-4000;
[0076] The density of the polypropylene used in the present invention is 0.90 g / cm 3 , melting point is 168°C, molecular weight is 2000-4000;
[0077] The vinyl-terminated T-type phenyl polysiloxane used in the present invention is purchased from Anhui IOTA Silicone Oil Co., Ltd., with a model of IOTA-253 and an ethylene content of 1.5-2.0 mmol / g.
[0078] Example 1
[0079] This embodiment provides a method for preparing a high-strength and flexible anti-electromagnetic interference shielding film, comprising the following steps:
[0080] S1. Preparation of modified adhesive
[0081] 2.4 g of 1,4-butenediol, 1.6 g of 1,6-hexamethylene diisocyanate and 18.0 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 70° C. and stirred for 2 h. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 80° C. and distilled under reduced pressure until no liquid was produced to obtain 3.5 g of modified polyurethane.
[0082] 3.2 g of modified polyurethane, 0.8 g of cyclopentanone, 10.7 g of N,N-dimethylformamide and 0.3 g of benzene were weighed and added into a reactor. The temperature of the reactor was raised to 70° C. After the reactor was cooled to room temperature, the reaction liquid was added into a rotary evaporator with a water bath temperature of 80° C. and distilled under reduced pressure until no liquid was produced, to obtain 3.8 g of hybrid polyurethane;
[0083] 3.3 g of hybrid polyurethane, 0.6 g of maleic anhydride, 12.0 g of N,N-dimethylformamide and 0.3 g of triethylamine were weighed and added to a reactor. The temperature of the reactor was raised to 40° C. and the reaction was kept warm for 2 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 100° C. and distilled under reduced pressure until no liquid was produced, to obtain 3.5 g of activated polyamide resin;
[0084] 3.2 g of activated polyurethane, 0.8 g of N,N'-di(2-naphthyl)-p-phenylenediamine, and 12.8 g of dimethyl sulfoxide were weighed and added to a reactor, and stirred at room temperature for 5 min. The temperature of the reactor was lowered to 0°C, and 0.2 g of 1-hydroxybenzotriazole and 0.2 g of dicyclohexylcarbodiimide were added thereto. The reaction was kept warm for 2 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 80°C, and distilled under reduced pressure until no liquid was produced, to obtain 3.8 g of amidated polyurethane;
[0085] Weigh 3.5 g of amidated polyurethane, 3.5 g of 4-cyclohexene-1,2-dicarboxylic acid diglycidyl ester, 1.3 g of vinyl-terminated T-phenyl polysiloxane, 0.1 g of azobisisobutyronitrile and 15.3 g of dimethyl sulfoxide and add them into a reactor. The temperature of the reactor is raised to 50°C and the reaction is kept warm for 2 hours. After the reactor is cooled to room temperature, the reaction liquid is added to a rotary evaporator with a water bath temperature of 80°C, and distilled under reduced pressure until no liquid is produced to obtain 8.1 g of a modified adhesive.
[0086] S2. Preparation of modified alloy
[0087] Weigh 6.4 g of Sendust magnetic powder and 0.6 g of multilayer graphene, add them into a grinder and grind them through a 300-mesh sieve to obtain 7.0 g of alloy powder;
[0088] 6.8 g of alloy powder, 28.3 g of deionized water, 0.01 g of chromic acid and 0.1 g of phosphoric acid were weighed and added to a reactor and stirred. The temperature of the reactor was raised to 80° C. and stirred until dry powder was obtained. The dry powder was placed in a drying oven at 200° C. and vacuum dried for 1 h to obtain 7.1 g of a modified alloy precursor.
[0089] 6.3 g of modified alloy precursor was placed in a -2 Into a 3000-ton ammonia nitriding furnace, high-purity ammonia was introduced, the gas pressure was maintained at 0.1 Torr, the temperature was raised to 500°C, the reaction was kept warm for 2 hours, and the sample chamber was gradually cooled to room temperature to obtain 6.4g of modified alloy.
[0090] S3. Preparation of organic membrane
[0091] 19.2 g of N,N'-dimethyloxamide, 4.8 g of hexafluorodianhydride, 64.0 g of dimethyl sulfoxide and 1.2 g of triethylamine were weighed and added to a reaction kettle, and stirred at room temperature for 2 h. After the reaction kettle was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 80°C, and distilled under reduced pressure until no liquid was produced, to obtain 23.5 g of modified polyamide resin;
[0092] 20.0 g of modified polyamide resin, 0.5 g of polypropylene, 0.5 g of styrene imine, 1.3 g of sodium alkylbenzene sulfonate, 0.8 g of nano-alumina and 60.0 g of dimethyl sulfoxide were weighed and added into a reaction kettle. The temperature of the reaction kettle was raised to 50° C. and stirred for 2 h to obtain 83.1 g of organic glue.
[0093] Pour 80.0g of organic glue into the electrospinning machine, set the voltage of the electrospinning machine to 20kV, set the spinning distance to 20cm, control the flow rate at 0.5L / h, and the spinning thickness to 15μm. After the spinning is completed, place the spinning product in a drying oven at 80℃ and vacuum dry it until the spinning product has a constant weight to obtain 22.5g of organic diaphragm layer.
[0094] S4. Preparation of anti-electromagnetic interference shielding film
[0095] 8.0 g of modified binder, 1.5 g of γ-aminopropyltriethoxysilane and 5.5 g of modified alloy were weighed and added to a grinder for grinding. After passing through a 300-mesh sieve, they were added to a reactor and stirred evenly to obtain 14.6 g of alloy powder.
[0096] The organic diaphragm layer obtained by the reaction is cut by a CNC cutting machine to obtain two square organic diaphragm layers with a side length of 200 mm;
[0097] 12.0g alloy powder, 1.2g sodium dodecyl sulfate, 0.8g polyethylene glycol, 12.0g 8wt% sodium hydroxide solution and 12.0g N,N-dimethylformamide were weighed and added into the extrusion coating machine pump. The slurry was applied to one side of two square organic diaphragm layers with a side length of 200mm through the extrusion port in a constant magnetic field of 20mT. The spin-coated surfaces of the two organic diaphragms were tightly fitted and dried at room temperature for 20h, and then put into a vulcanizer. The temperature of the vulcanizer was set to 180°C, the pressure was set to 5MPa, and the time was set to 3min to obtain an anti-electromagnetic interference diaphragm.
[0098] Example 2
[0099] This embodiment provides a method for preparing a high-strength and flexible anti-electromagnetic interference shielding film, comprising the following steps:
[0100] S1. Preparation of modified adhesive
[0101] 3.0 g of 1,4-butenediol, 2.0 g of 1,6-hexamethylene diisocyanate and 20.0 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 90° C. and stirred for 4 h. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 100° C. and distilled under reduced pressure until no liquid was produced to obtain 4.8 g of modified polyurethane.
[0102] 4.6 g of modified polyurethane, 1.2 g of cyclopentanone, 16.0 g of N,N-dimethylformamide and 0.4 g of benzene were weighed and added into a reactor. The temperature of the reactor was raised to 90° C. After the reactor was cooled to room temperature, the reaction liquid was added into a rotary evaporator with a water bath temperature of 100° C. and distilled under reduced pressure until no liquid was produced, to obtain 5.4 g of hybrid polyurethane;
[0103] 5.2 g of hybrid polyurethane, 0.8 g of maleic anhydride, 40.0 g of N,N-dimethylformamide and 0.4 g of triethylamine were weighed and added to a reactor. The temperature of the reactor was raised to 60° C. and the reaction was kept warm for 4 hours. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 100° C. and distilled under reduced pressure until no liquid was produced, to obtain 5.8 g of activated polyamide resin;
[0104] 5.4 g of activated polyurethane, 1.4 g of N,N'-di(2-naphthyl)-p-phenylenediamine, and 19.1 g of dimethyl sulfoxide were weighed and added to a reactor, and stirred at room temperature for 10 min. The temperature of the reactor was lowered to 5°C, and 0.4 g of 1-hydroxybenzotriazole and 0.4 g of dicyclohexylcarbodiimide were added thereto. The reaction was kept warm for 2 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 100°C, and distilled under reduced pressure until no liquid was produced, to obtain 6.4 g of amidated polyurethane;
[0105] 6.0 g of amidated polyurethane, 6.0 g of 4-cyclohexene-1,2-dicarboxylic acid diglycidyl ester, 3.0 g of vinyl-terminated T-type phenyl polysiloxane, 0.3 g of azobisisobutyronitrile and 24.0 g of dimethyl sulfoxide were weighed and added into a reactor. The temperature of the reactor was raised to 70°C and the reaction was kept warm for 4 hours. After the reactor was cooled to room temperature, the reaction liquid was added into a rotary evaporator with a water bath temperature of 100°C, and distilled under reduced pressure until no liquid was produced to obtain 14.6 g of a modified adhesive.
[0106] S2. Preparation of modified alloy
[0107] Weigh 14.9 g of Sendust magnetic powder and 1.1 g of multilayer graphene, add them into a grinder and grind them, and pass them through a 500-mesh sieve to obtain 16.0 g of alloy powder;
[0108] 15.8 g of alloy powder, 47.3 g of deionized water, 0.02 g of chromic acid and 0.4 g of phosphoric acid were weighed and added to a reactor and stirred. The temperature of the reactor was raised to 90° C. and stirred until dry powder was obtained. The dry powder was placed in a drying oven at 200° C. and vacuum dried for 2 h to obtain 16.2 g of a modified alloy precursor.
[0109] 15.0 g of modified alloy precursor was placed in a -3 Into a 3000-ton ammonia nitriding furnace, high-purity ammonia was introduced, the gas pressure was maintained at 0.5 Torr, the temperature was raised to 800°C, the reaction was kept warm for 3 hours, and the sample chamber was gradually cooled to room temperature to obtain 15.2g of modified alloy.
[0110] S3. Preparation of organic membrane
[0111] 18.5 g of N,N'-dimethyloxamide, 3.7 g of hexafluorodianhydride, 62.9 g of dimethyl sulfoxide and 1.5 g of triethylamine were weighed and added to a reaction kettle, and stirred at room temperature for 4 h. After the reaction kettle was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 80°C, and distilled under reduced pressure until no liquid was produced, to obtain 22.2 g of modified polyamide resin;
[0112] 21.0 g of modified polyamide resin, 0.7 g of polypropylene, 0.7 g of styrene imine, 1.5 g of sodium alkylbenzene sulfonate, 0.6 g of nano-alumina and 57.6 g of dimethyl sulfoxide were weighed and added into a reaction kettle. The temperature of the reaction kettle was raised to 60° C. and stirred for 3 h to obtain 82.1 g of organic glue.
[0113] Pour 80.0 organic glue into the electrospinning machine, set the voltage of the electrospinning machine to 25kV, the spinning distance to 30cm, the flow rate to 1L / h, the spinning thickness to 20μm, and after the spinning is completed, place the spinning product in a drying oven at 80℃ and vacuum dry it until the spinning product has a constant weight, to obtain 23.1g of organic diaphragm layer.
[0114] S4. Preparation of anti-electromagnetic interference shielding film
[0115] 8.0 g of modified binder, 2.0 g of γ-aminopropyltriethoxysilane and 6.0 g of modified alloy were weighed and added to a grinder for grinding. After passing through a 300-mesh sieve, they were added to a reaction kettle and stirred evenly to obtain 16.0 g of alloy powder.
[0116] The organic diaphragm layer obtained by the reaction is cut by a CNC cutting machine to obtain two square organic diaphragm layers with a side length of 200 mm;
[0117] 14.0g alloy powder, 1.4g sodium dodecyl sulfate, 0.7g polyethylene glycol, 12.0g 16wt% sodium hydroxide solution and 14.0g N,N-dimethylformamide were weighed and added to the extrusion coater pump. The slurry was applied to one side of two square organic diaphragm layers with a side length of 200mm through the extrusion port in a constant magnetic field of 40mT. The spin-coated surfaces of the two organic diaphragms were tightly fitted and dried at room temperature for 24h, and then put into a vulcanizer. The temperature of the vulcanizer was set to 200℃, the pressure was set to 10MPa, and the time was set to 5min to obtain an anti-electromagnetic interference diaphragm.
[0118] Example 3
[0119] This embodiment provides a method for preparing a high-strength and flexible anti-electromagnetic interference shielding film, comprising the following steps:
[0120] S1. Preparation of modified adhesive
[0121] 2.4 g of 1,4-butenediol, 1.6 g of 1,6-hexamethylene diisocyanate and 18.0 g of N,N-dimethylformamide were weighed and added to a reactor. The temperature of the reactor was raised to 80° C. and stirred for 3 h. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 90° C. and distilled under reduced pressure until no liquid was produced to obtain 3.6 g of modified polyurethane;
[0122] 3.0 g of modified polyurethane, 1.2 g of cyclopentanone, 13.5 g of N,N-dimethylformamide and 0.3 g of benzene were weighed and added into a reactor. The temperature of the reactor was raised to 80° C. After the reactor was cooled to room temperature, the reaction liquid was added into a rotary evaporator with a water bath temperature of 90° C. and distilled under reduced pressure until no liquid was produced, to obtain 4.0 g of hybrid polyurethane;
[0123] 3.6 g of hybrid polyurethane, 0.6 g of maleic anhydride, 12.0 g of N,N-dimethylformamide and 0.3 g of triethylamine were weighed and added to a reactor. The temperature of the reactor was raised to 50° C. and the reaction was kept warm for 3 hours. After the reactor was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 90° C. and distilled under reduced pressure until no liquid was produced, to obtain 4.0 g of activated polyamide resin;
[0124] 3.6 g of activated polyurethane, 1.2 g of N,N'-di(2-naphthyl)-p-phenylenediamine, and 13.5 g of dimethyl sulfoxide were weighed and added to a reactor, and stirred at room temperature for 8 min. The temperature of the reactor was lowered to 3°C, and 0.2 g of 1-hydroxybenzotriazole and 0.2 g of dicyclohexylcarbodiimide were added thereto. The reaction was kept warm for 2 h. After the reactor was cooled to room temperature, the reaction solution was added to a rotary evaporator with a water bath temperature of 90°C, and distilled under reduced pressure until no liquid was produced, to obtain 4.5 g of amidated polyurethane;
[0125] 4.1 g of amidated polyurethane, 4.1 g of 4-cyclohexene-1,2-dicarboxylic acid diglycidyl ester, 1.8 g of vinyl-terminated T-phenyl polysiloxane, 0.2 g of azobisisobutyronitrile and 15.9 g of dimethyl sulfoxide were weighed and added into a reactor. The temperature of the reactor was raised to 60°C and the reaction was kept warm for 3 hours. After the reactor was cooled to room temperature, the reaction liquid was added into a rotary evaporator with a water bath temperature of 90°C, and distilled under reduced pressure until no liquid was produced to obtain 9.6 g of modified adhesive.
[0126] S2. Preparation of modified alloy
[0127] Weigh 5.8 g of Sendust magnetic powder and 0.4 g of multilayer graphene, add them into a grinder and grind them through a 400-mesh sieve to obtain 6.2 g of alloy powder;
[0128] Weigh 6.2 g of alloy powder, 20.8 g of deionized water, 0.01 g of chromic acid and 0.16 g of phosphoric acid, add them into a reactor and stir, raise the temperature of the reactor to 90° C., stir until dry powder is in a state, place the dry powder in a drying oven at 200° C. and vacuum dry for 2 h to obtain 6.3 g of modified alloy precursor;
[0129] 6.0 g of modified alloy precursor was placed in a -3 Into a 3000-ton ammonia nitriding furnace, high-purity ammonia was introduced, the gas pressure was maintained at 0.3 Torr, the temperature was raised to 650°C, the reaction was kept warm for 3 hours, and the sample chamber was gradually cooled to room temperature to obtain 6.2g of modified alloy.
[0130] S3. Preparation of organic membrane
[0131] 21.0 g of N,N'-dimethyloxamide, 5.0 g of hexafluorodianhydride, 85.0 g of dimethyl sulfoxide and 2.4 g of triethylamine were weighed and added to a reaction kettle, and stirred at room temperature for 3 h. After the reaction kettle was cooled to room temperature, the reaction liquid was added to a rotary evaporator with a water bath temperature of 90°C, and distilled under reduced pressure until no liquid was produced, to obtain 25.3 g of modified polyamide resin;
[0132] 24.0 g of modified polyamide resin, 0.6 g of polypropylene, 0.6 g of styrene imine, 1.5 g of sodium alkylbenzene sulfonate, 1.0 g of nano-alumina particles and 60.0 g of dimethyl sulfoxide were weighed and added into a reaction kettle. The temperature of the reaction kettle was raised to 55° C. and stirred for 3 h to obtain 87.7 g of organic glue.
[0133] Pour 85.0g of organic glue into the electrospinning machine, set the voltage of the electrospinning machine to 23kV, set the spinning distance to 25cm, control the flow rate at 0.75L / h, and the spinning thickness to 18μm. After the spinning is completed, place the spinning product in a drying oven at 80°C and vacuum dry it until the spinning product has a constant weight, obtaining 25.3g of an organic diaphragm layer.
[0134] S4. Preparation of anti-electromagnetic interference shielding film
[0135] 9.0 g of modified binder, 2.0 g of γ-aminopropyltriethoxysilane and 6.0 g of modified alloy were weighed and added to a grinder for grinding. After passing through a 300-mesh sieve, they were added to a reaction kettle and stirred evenly to obtain 17.0 g of alloy powder.
[0136] The organic diaphragm layer obtained by the reaction is cut by a CNC cutting machine to obtain two square organic diaphragm layers with a side length of 200 mm;
[0137] 12.0g alloy powder, 1.4g sodium dodecyl sulfate, 0.9g polyethylene glycol, 14.0g 12wt% sodium hydroxide solution and 10.0g N,N-dimethylformamide were weighed and added to the extrusion coater pump. The slurry was applied to one side of two square organic diaphragm layers with a side length of 200mm through the extrusion port in a constant magnetic field of 30mT. The spin-coated surfaces of the two organic diaphragms were tightly fitted and dried at room temperature for 24h, and then put into a vulcanizer. The temperature of the vulcanizer was set to 190°C, the pressure was set to 8MPa, and the time was set to 5min to obtain an anti-electromagnetic interference diaphragm.
[0138] Comparative Example 1
[0139] The difference between this comparative example and Example 3 is that the preparation of hybrid polyurethane in step S1 and subsequent steps are eliminated, and in step S4, an equal amount of modified polyurethane is used to replace the modified adhesive.
[0140] Comparative Example 2
[0141] The difference between this comparative example and Example 3 is that step S2 is eliminated, and in step S4, an equal amount of sendust magnetic powder is used to replace the modified alloy.
[0142] Comparative Example 3
[0143] The difference between this comparative example and Example 3 is that step S3 is eliminated, and in step S4, an equal amount of polyvinyl chloride membrane is used to replace the organic membrane layer.
[0144] Performance Test:
[0145] The shielding effectiveness, electrical properties, tensile strength, tensile modulus, flexural strength, flexural modulus impact strength (with notch) and high temperature resistance of a high-strength flexible anti-electromagnetic interference shielding film prepared in Examples 1-3 and Comparative Examples 1-3 were tested with reference to the standard GB / T 32511-2016 "General Technical Requirements for Electromagnetic Shielding Plastics". The specific test results are shown in Table 1:
[0146] Table 1-Test data table of each test sample
[0147]
[0148]
[0149] Data Analysis:
[0150] Comparative analysis of the data in Table 1 above shows that the high-strength and flexible anti-electromagnetic interference shielding film prepared by the present invention has an anti-electromagnetic interference level of SE-1, an electrical performance level of EP-1, a mechanical performance level of MP-1, and a thermal performance level of HOT-1, and all performance test data are better than those of the comparative example;
[0151] It is explained that the present invention obtains a modified polyurethane by polymerizing 1,4-butenediol and 1,6-hexamethylene diisocyanate, reduces side reactions and introduces double bonds by hybridization, further activates and introduces double bonds while increasing the active functional group hydroxyl group, further enhances the high temperature resistance of the product by amidation, and finally obtains a modified adhesive by free radical polymerization. During the polymerization, the abundant double bonds inside the amidated polyurethane give the adhesive a more complex spatial structure, further improving its bonding ability, and the abundant epoxy groups inside give it flexibility while enhancing its toughness.
[0152] Furthermore, the electromagnetic shielding performance of the modified alloy obtained by nitriding after crushing and mixing sendust and multilayer graphene to form a phosphorus-coated core-shell structure is further enhanced, and its bonding force with the adhesive is further enhanced. Furthermore, a modified polyamide resin is obtained by polymerizing N,N'-dimethyloxamide and hexafluorodianhydride, and its bonding force with the adhesive is enhanced by combining its internal carboxyl group with the epoxy group of the adhesive, and its abundant internal fluorine groups further improve its heat resistance;
[0153] In summary, the present invention prepares a modified polyurethane and obtains an adhesive through hybridization, activation, amidation and free radical polymerization reaction, and then uses its mixed modified alloy to bond with an organic diaphragm prepared by the present invention to obtain an anti-electromagnetic interference shielding film with strong electromagnetic resistance, high flexibility, high temperature resistance and high mechanical properties.
[0154] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0155] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0156] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A high-strength and flexible anti-electromagnetic interference shielding film, It is characterized in that It comprises an alloy skeleton layer (100), the exterior of which is coated with an organic diaphragm layer (200); The composite skeleton layer (100) is obtained by coating a mixture of a modified adhesive and a modified alloy and curing the mixture on the surface of the organic diaphragm layer, and the organic diaphragm layer (200) is obtained by processing a modified polyamide resin.
2. A high-strength and flexible anti-electromagnetic interference shielding film according to claim 1, It is characterized in that The preparation method of the modified adhesive is as follows: 8-10 parts of amidated polyurethane, 8-10 parts of 4-cyclohexene-1,2-dicarboxylic acid diglycidyl ester, 3-5 parts of vinyl-terminated T-phenyl polysiloxane, 0.3-0.5 parts of azobisisobutyronitrile and 30-40 parts of dimethyl sulfoxide are weighed by weight and added into a reaction kettle, the temperature of the reaction kettle is increased to 50-70°C, the reaction is kept warm for 2-4 hours, and the modified adhesive is obtained by post-treatment.
3. A high-strength and flexible anti-electromagnetic interference shielding film according to claim 2, It is characterized in that The preparation method of amidated polyurethane is as follows: 20-30 parts of activated polyurethane, 5-10 parts of N,N'-di(2-naphthyl)-p-phenylenediamine and 75-100 parts of dimethyl sulfoxide are weighed by weight and added into a reaction kettle, stirred at room temperature for 5-10 minutes, the temperature of the reaction kettle is lowered to 0-5°C, 1-2 parts of 1-hydroxybenzotriazole and 1-2 parts of dicyclohexylcarbodiimide are added thereto, the reaction is kept warm for 1-2 hours, and the amidated polyurethane is obtained by post-treatment.
4. A high-strength and flexible anti-electromagnetic interference shielding film according to claim 3, It is characterized in that The preparation method of activated polyurethane is as follows: 20-30 parts of hybrid polyurethane, 3-5 parts of maleic anhydride, 75-100 parts of N,N-dimethylformamide and 1-3 parts of triethylamine are weighed and added into a reaction kettle, the temperature of the reaction kettle is increased to 40-60°C, the reaction is kept warm for 2-4 hours, and the activated polyamide resin is obtained by post-treatment.
5. A high-strength and flexible anti-electromagnetic interference shielding film according to claim 4, It is characterized in that The preparation method of hybrid polyurethane is as follows: 20-30 parts of modified polyurethane, 5-10 parts of cyclopentanone, 75-100 parts of N,N-dimethylformamide and 1-3 parts of benzene are weighed and added into a reaction kettle, the temperature of the reaction kettle is raised to 70-90° C., and the hybrid polyurethane is obtained by post-treatment.
6. A high-strength and flexible anti-electromagnetic interference shielding film according to claim 5, It is characterized in that The preparation method of the modified polyurethane is as follows: 5-8 parts of 1,4-butene diol, 4-6 parts of 1,6-hexamethylene diisocyanate and 40-50 parts of N,N-dimethylformamide are weighed by weight and added into a reaction kettle, the temperature of the reaction kettle is increased to 70-90°C, the mixture is stirred for 2-4 hours, and the modified polyurethane is obtained by post-treatment.
7. A high-strength and flexible anti-electromagnetic interference shielding film according to claim 1, It is characterized in that The preparation method of the modified alloy comprises the following steps: A1. Weigh 20-30 parts of Sendust magnetic powder and 2-3 parts of multilayer graphene by weight, add them into a pulverizer and grind them, and pass them through a 300-500 mesh sieve to obtain alloy powder; A2, weighing 10-20 parts of alloy powder, 40-60 parts of deionized water, 0.01-0.02 parts of chromic acid and 0.2-0.4 parts of phosphoric acid by weight, adding them into a reactor and stirring, raising the temperature of the reactor to 80-90° C., stirring until dry powder state, and post-treating to obtain a modified alloy precursor; A3. Place the modified alloy precursor in a -2 -10 -3 Into a 300-4000 ton ammonia nitriding furnace, high-purity ammonia is introduced, the gas pressure is maintained at 0.1-0.5 Torr, the temperature is raised to 500-800°C, the reaction is kept at this temperature for 2-3 hours, and the sample chamber is gradually cooled to room temperature to obtain a modified alloy.
8. A high-strength and flexible anti-electromagnetic interference shielding film according to claim 1, It is characterized in that The preparation method of the modified polyamide resin is as follows: 20-30 parts of N,N'-dimethyloxamide, 5-10 parts of hexafluorodianhydride, 75-100 parts of dimethyl sulfoxide and 1-3 parts of triethylamine are weighed and added into a reaction kettle, stirred at room temperature for 2-4 hours, and post-treated to obtain the modified polyamide resin.
9. A high-strength and flexible anti-electromagnetic interference shielding film according to claim 1, It is characterized in that The method for preparing the organic diaphragm layer comprises the following steps: B1. 80-100 parts of modified polyamide resin, 2-3 parts of reinforcing agent, 2-3 parts of antioxidant, 5-8 parts of wetting agent, 1-5 parts of filler and 200-300 parts of dimethyl sulfoxide are weighed and added into a reaction kettle. The temperature of the reaction kettle is raised to 50-60° C. and stirred for 2-3 hours to obtain an organic glue solution. B2. Pour the organic glue into an electrospinning machine, set the voltage of the electrospinning machine to 20-25 kV, set the spinning distance to 20-30 cm, control the flow rate to 0.5-1 L / h, and the spinning thickness to 15-20 μm, and post-treat to obtain an organic diaphragm layer.
10. A method for preparing a high-strength and flexible anti-electromagnetic interference shielding film according to any one of claims 1 to 9, It is characterized in that The following steps are involved: S1. Weigh 8-10 parts of modified binder, 1-2 parts of γ-aminopropyltriethoxysilane and 5-8 parts of modified alloy by weight, add them into a pulverizer and grind them. After passing through a 300-mesh sieve, add them into a reaction kettle and stir them evenly to obtain alloy powder. S2, cutting the organic diaphragm layer obtained by the reaction by a CNC cutting machine to obtain two square organic diaphragm layers with a side length of 200 mm; S3. Weigh 20-30 parts of alloy powder, 2-3 parts of sodium dodecyl sulfate, 1-2 parts of polyethylene glycol, 20-30 parts of 8-16wt% sodium hydroxide solution and 20-30 parts of N,N-dimethylformamide by weight and add them to the extrusion coating machine pump. Apply the slurry to one side of two square organic diaphragm layers with a side length of 200 mm through the extrusion port in a constant magnetic field of 20-40mT. Put the spin-coated surfaces of the two organic diaphragms tightly together and dry them at room temperature for 20-24h, then put them into a vulcanizer. Set the temperature of the vulcanizer to 180-200℃, the pressure to 5-10MPa, and the time to 3-5min to obtain an anti-electromagnetic interference diaphragm.
Citation Information
Patent Citations
Electromagnetic wave interference suppression coating
CN110484110A
Polyimide-based electromagnetic shielding film with sandwich structure and preparation method of polyimide-based electromagnetic shielding film
CN113913952A
FPC electromagnetic shielding film with polyimide film as insulating layer, and preparation method therefor
WO2020020195A1