Copper embossment and processing technology thereof
By using copper relief composed of substrate layer, adhesive layer and embossing layer, combined with specific adhesive and polishing agent formulas, the existing embossing materials have been solved, and the high copper relief is achieved Plasticity, hardness and fire resistance to meet modern decoration needs.
Patent Information
- Application Number
- CN202411192794.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-26
AI Technical Summary
The existing relief materials have problems such as poor fire resistance, poor environmental protection, short service life and fragility in building decoration, and the process is complicated, making it difficult to meet the needs of modern decoration.
Copper relief consisting of substrate layer, adhesive layer and embossing layer. The embossing layer consists of acrylic resin, sodium silicate solution, calcium carbonate, talc powder, aluminum hydroxide powder, etc., and covers the surface with copper skin, through specific Adhesive and polishing agent formulations improve bond strength and water resistance and are rolled through three-dimensional pattern molds.
The high plasticity, hardness and fire resistance of copper relief are achieved, and the glue strength and water resistance are improved. At the same time, the polishing agent ensures the brightness and environmental protection of the metal surface, avoiding rust and dirt residue.
Smart Images

Figure CN119017862A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of relief preparation, in particular to a copper relief and a processing technology thereof. Background Art
[0002] As a unique decorative material, relief originated from the influence of ancient art and architecture, and its history can be traced back to human civilization thousands of years ago. Early relief art craftsmen used stone, wood and metal to create exquisite three-dimensional effects through hand-carving techniques. With the advent of the Industrial Revolution, the emergence of new materials and production processes has gradually industrialized the manufacture of reliefs. Modern reliefs are usually made of polymer materials, fiber cement, wood-plastic composite materials, etc., and are produced through technologies such as molding, injection molding or 3D printing, which not only reduces costs, but also improves production efficiency and design flexibility. The wide application of relief covers areas such as building exterior wall decoration, interior wall design, furniture manufacturing and advertising signs, adding rich visual layers and artistic atmosphere to architectural and space design.
[0003] At present, relief decoration is often used in building decoration. The relief surface has an uneven wooden three-dimensional texture pattern. It is mainly milled and polished on the surface of the wooden board with a wire roller. However, it is limited by the variety of wooden boards and does not have fire resistance. It is not environmentally friendly and wastes resources. Relief boards made of other materials, such as gypsum relief boards, have the disadvantages of short service life, low plasticity, fragility and mildew. For example, Chinese patent document CN201610799370.5 discloses a rubber mud relief decorative board and its manufacturing process. By using rubber mud to adhere to the surface of the substrate, the construction is complicated and the fire resistance is poor. At the same time, there is a problem of moisture and shedding. Summary of the invention
[0004] In view of the deficiencies in the prior art, the object of the present invention is to provide a copper relief and a processing technology thereof.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A copper relief, the copper relief is composed of a substrate layer, an adhesive layer and a relief layer, the surface of the relief layer is covered with a layer of copper skin, the relief layer comprises the following raw materials: 10-20 parts of acrylic resin, 5-10 parts of sodium silicate solution, 20-30 parts of calcium carbonate, 10-20 parts of talcum powder, 15-25 parts of aluminum hydroxide powder, 1-3 parts of sodium carboxymethyl cellulose, 0.2-0.4 parts of defoaming agent, 0.5-1 parts of dispersant;
[0007] The bonding layer is an adhesive layer, and the preparation method of the adhesive is as follows: dissolving carboxymethyl chitosan in deionized water, then adding guanidine sulfamate and epichlorohydrin thereto, stirring to react, and after the reaction is completed, cooling to room temperature, then adding sodium polyphosphate solution, stirring for 30-60 minutes, and then adding zinc salt solution, and continuing to stir for 1-2 hours to obtain the adhesive.
[0008] Specifically, the mass ratio of the carboxymethyl chitosan, deionized water, guanidine sulfamate, epichlorohydrin, sodium polyphosphate solution and zinc salt solution is 8-12:100-150:4-6:5-8:20-30:10-20.
[0009] Specifically, the mass fraction of the sodium polyphosphate solution is 10-20%.
[0010] Specifically, the mass fraction of the zinc salt solution is 5-10%.
[0011] Specifically, the stirring reaction temperature is 50-80° C., and the stirring reaction time is 3-5 h.
[0012] Specifically, the mass fraction of the sodium silicate solution is 10-20%.
[0013] The present invention also provides a processing technology for the copper relief, comprising the following steps:
[0014] S1. Evenly coating the prepared adhesive on the surface of the substrate layer to obtain an adhesive layer;
[0015] S2, adding acrylic resin, sodium silicate solution, sodium carboxymethyl cellulose, defoamer and dispersant into a container by weight, stirring and mixing evenly to obtain slurry, then pouring the slurry into a kneader, and pouring calcium carbonate, talcum powder and aluminum hydroxide powder into the kneader, kneading for 3-5 minutes to obtain a soft mud material;
[0016] S3, rolling the soft mud material into a relief layer film with a thickness of 1-10mm, and spreading it on the bonding layer, then rolling the surface of the relief layer film with a three-dimensional pattern mold roller to form a three-dimensional pattern to obtain a relief layer, and after drying, a layer of red copper skin is covered on the surface of the relief layer to obtain a copper relief.
[0017] Specifically, in step S1, the coating amount of the adhesive is 150-200 g / m 2 .
[0018] Specifically, in step S3, the thickness of the copper skin is 0.1-0.3 mm.
[0019] Specifically, the method also includes polishing the surface of the copper relief. The selected polishing agent includes the following raw materials: 80-100 parts of hydrogen peroxide, 30-40 parts of sodium phosphate, 10-15 parts of disodium ethylenediaminetetraacetic acid, 10-15 parts of 5-aminosalicylic acid, 3-5 parts of nano silicon dioxide, 8-10 parts of alkylphenol polyoxyethylene ether, and 5-10 parts of sodium lignin sulfonate.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) The copper relief prepared by the present invention has good plasticity and is easy to shape; the present invention uses acrylic resin and sodium silicate solution as two components as the glue, so that the overall structure of the product is harder and stronger, and it is not easy to deform and crack under natural conditions.
[0022] (2) The present invention grafts guanidine aminosulfonate onto carboxymethyl chitosan through the cross-linking effect of epichlorohydrin. By modifying the carboxymethyl chitosan, the spatial network structure of the carboxymethyl chitosan molecule is increased. At the same time, the amino group in guanidine aminosulfonate is positively charged and the sodium polyphosphate is negatively charged. The electrostatic effect increases the cross-linking degree of the reaction system, making the molecular network structure more stable, thereby improving the bonding strength and water resistance of the adhesive. At the same time, the added zinc ions can coordinate with the amino groups in guanidine aminosulfonate to form a coordination compound. The molecular chains in the network structure are connected by coordination bonds, further increasing the cross-linking density, effectively preventing water swelling, and further improving the bonding strength and water resistance of the adhesive. In addition, the guanidine aminosulfonate in the adhesive has excellent flame retardant properties, which work together with the zinc ions to improve the flame retardant properties of the adhesive.
[0023] (3) The polishing agent provided by the present invention can effectively improve the brightness of the metal surface without leaving any residue, thus ensuring the purity and safety of the product; at the same time, the polishing effect of the polishing agent is very stable, which can not only effectively remove dirt and oxides on the metal surface, but also prevent metal products from rusting due to environmental factors. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The schematic diagram of the structure of the copper relief prepared by the present invention. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.
[0026] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.
[0027] A copper relief processing technology comprises the following steps:
[0028] S1. Evenly coat the prepared adhesive on the surface of the substrate layer to obtain an adhesive layer.
[0029] In this step, the substrate layer selected is a wood board or a gypsum board.
[0030] In this step, the preparation method of the adhesive is as follows: dissolve carboxymethyl chitosan in deionized water, then add guanidine sulfamate and epichlorohydrin thereto, stir to react, after the reaction is completed, cool to room temperature, then add sodium polyphosphate solution, stir for 30-60 minutes, then add zinc salt solution, continue stirring for 1-2 hours, and obtain the adhesive.
[0031] Specifically, the mass ratio of carboxymethyl chitosan, deionized water, guanidine sulfamate, epichlorohydrin, sodium polyphosphate solution and zinc salt solution is 8-12:100-150:4-6:5-8:20-30:10-20, and more preferably 9-10:120-130:4.5-5:6-7:24-26:14-16.
[0032] More specifically, the mass fraction of the sodium polyphosphate solution is 10-20%. In some embodiments of the present invention, for example, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, and 20% can be selected, but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] The mass fraction of the zinc salt solution is 5-10%. In some embodiments of the present invention, for example, 5%, 6%, 7%, 8%, 9%, and 10% may be selected, but it is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0034] Wherein, the zinc salt is selected from soluble zinc salts, for example, zinc chloride, zinc nitrate or zinc sulfate.
[0035] Specifically, the stirring reaction temperature is 50-80°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, and 80°C can be selected; the stirring reaction time is 3-5h, for example, 3h, 3.5h, 4h, 4.5h, and 5h can be selected; but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] In this step, the coating amount of adhesive is 150-200g / m 2 For example, you can choose 150g / m 2 , 160g / m 2 , 170g / m 2 , 180g / m 2 , 190g / m 2, 200g / m 2 , but not limited to the listed values, other unlisted values within the numerical range are also applicable.
[0037] S2. Add acrylic resin, sodium silicate solution, sodium carboxymethyl cellulose, defoamer and dispersant into a container according to weight, stir and mix evenly to obtain slurry, then pour the slurry into a kneader, and pour calcium carbonate, talcum powder and aluminum hydroxide powder into the kneader, knead for 3-5 minutes to obtain a soft mud material.
[0038] In this step, the acrylic resin can be selected from 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, and 20 parts; but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0039] The sodium silicate solution can be selected to be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, and 10 parts, wherein the mass fraction of the sodium silicate solution is 10-20%, for example, 10%, 12%, 14%, 15%, 16%, 18%, 19%, 20% can be selected, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0040] Calcium carbonate can be selected as 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, and 30 parts, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] The particle size of calcium carbonate is 40-80 nm, more preferably 60 nm.
[0042] The talc powder can be selected in 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts; but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0043] The mesh size of talc is 325-800 mesh, more preferably 400 mesh.
[0044] The aluminum hydroxide powder can be selected in 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0045] The mesh size of the aluminum hydroxide powder is 1250-4000 mesh, and more preferably 2000 mesh.
[0046] The amount of sodium carboxymethyl cellulose can be 1 part, 1.5 parts, 2 parts, 2.5 parts, or 3 parts, but is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0047] The defoaming agent can be selected as 0.2 parts, 0.3 parts, or 0.4 parts, but is not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0048] Specifically, the defoamer is selected from mineral oil defoamers, preferably polyether-modified siloxane.
[0049] The dispersant can be selected from 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, and 1 part, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0050] Specifically, the dispersant is selected from anionic dispersants, preferably dispersant SN-5040.
[0051] S3, rolling the soft mud material into a relief layer film with a thickness of 1-10mm, and spreading it on the bonding layer, then rolling the surface of the relief layer film with a three-dimensional pattern mold roller to form a three-dimensional pattern to obtain a relief layer, and after drying, a layer of red copper skin is covered on the surface of the relief layer to obtain a copper relief.
[0052] In this step, the drying is preferably natural drying.
[0053] The thickness of the copper skin is 0.1-0.3 mm, for example, 0.1 mm, 0.2 mm, 0.3 mm can be selected, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0054] In addition, this step also includes polishing the surface of the copper relief, and the selected polishing agent includes the following raw materials: 80-100 parts of hydrogen peroxide, 30-40 parts of sodium phosphate, 10-15 parts of disodium ethylenediaminetetraacetic acid, 10-15 parts of 5-aminosalicylic acid, 3-5 parts of nano silicon dioxide, 8-10 parts of alkylphenol polyoxyethylene ether, and 5-10 parts of sodium lignin sulfonate.
[0055] Hydrogen peroxide is a highly effective oxidant that can help remove dirt and oxides from metal surfaces; it can also remove excess grease and dirt from the metal surface, thus preparing it for the subsequent polishing step.
[0056] Sodium phosphate mainly acts as a buffer, which can help stabilize the pH value of the solution; at the same time, it also acts as a surfactant, promoting the emulsification of oil and impurities, thereby improving the cleaning effect.
[0057] As a chelating agent, disodium EDTA can effectively combine with metal ions to prevent them from precipitating or settling on the metal surface; by removing metal ions, it can effectively reduce the corrosion of the metal surface and make the polishing effect more prominent.
[0058] 5-Aminosalicylic acid is an organic acid with good ability to remove rust and oxides; it promotes the cleaning and smoothing of metal surfaces through chemical reactions, helping to improve the gloss effect during polishing.
[0059] The tiny particles of nano-silicon dioxide can enter the tiny pits on the metal surface, effectively removing surface unevenness and thus improving the gloss of the metal.
[0060] As surfactants, alkylphenol polyoxyethylene ether and sodium lignin sulfonate have good dispersing properties, which can help remove impurities and dust from the metal surface. At the same time, they can also improve the lubrication properties of the polishing agent and help reduce possible scratches during the polishing process.
[0061] The present invention is further illustrated by specific examples below. The brand of acrylic resin is JE-6132, purchased from Changzhou Gene New Materials Co., Ltd.; the mass fraction of sodium silicate solution is 15%; the particle size of calcium carbonate is 60nm; the mesh number of talc powder is 400 mesh; the mesh number of aluminum hydroxide powder is 2000 mesh; the defoaming agent is polyether-modified heptamethyl trisiloxane, CAS No.: 27306-78-1; and the model of dispersant is dispersant SN-5040.
[0062] Example 1
[0063] A copper relief processing technology comprises the following steps:
[0064] S1, 10g of carboxymethyl chitosan was dissolved in 100g of deionized water, and then 4g of guanidine sulfamate and 5g of epichlorohydrin were added thereto, and the reaction was stirred at 50°C for 5h. After the reaction was completed, it was cooled to room temperature, and then 20g of 10wt% sodium polyphosphate solution was added, stirred for 30min, and then 10g of 5wt% zinc nitrate solution was added, and stirring was continued for 1h to obtain an adhesive;
[0065] S2. Use a glue coating machine to evenly roll the prepared adhesive onto the surface of the substrate layer. The selected substrate layer is eucalyptus board, and the coating amount of the adhesive is 150g / m 2 ;
[0066] S3, 10 parts of acrylic resin, 5 parts of sodium silicate solution, 1 part of sodium carboxymethyl cellulose, 0.2 parts of defoaming agent and 0.5 parts of dispersant are added to a container, stirred and mixed evenly to obtain a slurry, and then the slurry is poured into a kneader, and 20 parts of calcium carbonate, 10 parts of talc and 15 parts of aluminum hydroxide powder are poured into the kneader, kneaded for 5 minutes, and a soft mud material is obtained;
[0067] S4. Use a flat roller to roll the soft mud into a relief layer film with a thickness of 5 mm, and spread it flat on the bonding layer. Then use a three-dimensional pattern mold roller to roll the surface of the relief layer film to form a three-dimensional pattern to obtain a relief layer. After natural drying, cover the surface of the relief layer with a 0.1 mm thick copper sheet to obtain a copper relief.
[0068] Example 2
[0069] A copper relief processing technology comprises the following steps:
[0070] S1, 12g carboxymethyl chitosan was dissolved in 150g deionized water, and then 6g guanidine sulfamate and 8g epichlorohydrin were added thereto, and the reaction was stirred at 80°C for 3h. After the reaction was completed, it was cooled to room temperature, and then 30g of 10wt% sodium polyphosphate solution was added, stirred for 30min, and then 20g of 5wt% zinc nitrate solution was added, and stirring was continued for 1h to obtain an adhesive;
[0071] S2. Use a glue coating machine to evenly roll the prepared adhesive onto the surface of the substrate layer, where the selected substrate layer is eucalyptus board, and the coating amount of the adhesive is 200g / m 2 ;
[0072] S3, 20 parts of acrylic resin, 10 parts of sodium silicate solution, 3 parts of sodium carboxymethyl cellulose, 0.4 parts of defoaming agent and 1 part of dispersant are added to a container, stirred and mixed evenly to obtain a slurry, and then the slurry is poured into a kneader, and 30 parts of calcium carbonate, 20 parts of talc and 25 parts of aluminum hydroxide powder are poured into the kneader, kneaded for 5 minutes, and a soft mud material is obtained;
[0073] S4. Use a flat roller to roll the soft mud into a relief layer film with a thickness of 8 mm, and spread it flat on the bonding layer. Then use a three-dimensional pattern mold roller to roll the surface of the relief layer film to form a three-dimensional pattern to obtain a relief layer. After natural drying, cover the surface of the relief layer with a 0.2 mm thick copper sheet to obtain a copper relief.
[0074] Example 3
[0075] A copper relief processing technology comprises the following steps:
[0076] S1, 10g carboxymethyl chitosan was dissolved in 150g deionized water, and then 5g guanidine sulfamate and 6g epichlorohydrin were added thereto, and the reaction was stirred at 60°C for 4h. After the reaction was completed, it was cooled to room temperature, and then 25g of 20wt% sodium polyphosphate solution was added, stirred for 45min, and then 10g of 10wt% zinc nitrate solution was added, and stirring was continued for 1h to obtain an adhesive;
[0077] S2. Use a glue coating machine to evenly roll the prepared adhesive onto the surface of the substrate layer. The selected substrate layer is eucalyptus board, and the coating amount of the adhesive is 180g / m 2 ;
[0078] S3, 16 parts of acrylic resin, 8 parts of sodium silicate solution, 2 parts of sodium carboxymethyl cellulose, 0.3 parts of defoaming agent and 0.6 parts of dispersant are added to a container, stirred and mixed evenly to obtain a slurry, and then the slurry is poured into a kneader, and 25 parts of calcium carbonate, 15 parts of talc and 20 parts of aluminum hydroxide powder are poured into the kneader, kneaded for 5 minutes, and a soft mud material is obtained;
[0079] S4. Use a flat roller to roll the soft mud into a relief layer film with a thickness of 4 mm, and spread it flat on the bonding layer. Then use a three-dimensional pattern mold roller to roll the surface of the relief layer film to form a three-dimensional pattern to obtain a relief layer. After natural drying, cover the surface of the relief layer with a 0.3 mm thick copper sheet to obtain a copper relief.
[0080] Example 4
[0081] A copper relief processing technology comprises the following steps:
[0082] S1, 8g of carboxymethyl chitosan was dissolved in 150g of deionized water, and then 6g of guanidine sulfamate and 5g of epichlorohydrin were added thereto, and the reaction was stirred at 60°C for 4h. After the reaction was completed, it was cooled to room temperature, and then 30g of 15wt% sodium polyphosphate solution was added, stirred for 60min, and then 15g of 5wt% zinc nitrate solution was added, and stirring was continued for 2h to obtain an adhesive;
[0083] S2. Use a glue coating machine to evenly roll the prepared adhesive onto the surface of the substrate layer. The selected substrate layer is eucalyptus board, and the coating amount of the adhesive is 160g / m 2 ;
[0084] S3, 15 parts of acrylic resin, 6 parts of sodium silicate solution, 2 parts of sodium carboxymethyl cellulose, 0.4 parts of defoaming agent and 0.8 parts of dispersant are added to a container, stirred and mixed evenly to obtain a slurry, and then the slurry is poured into a kneader, and 24 parts of calcium carbonate, 16 parts of talc and 18 parts of aluminum hydroxide powder are poured into the kneader, kneaded for 5 minutes, and a soft mud material is obtained;
[0085] S4. The soft mud material is rolled into a 6 mm thick relief layer film by using a flat roller, and is spread flat on the bonding layer. The surface of the relief layer film is then rolled with a three-dimensional pattern mold roller to form a three-dimensional pattern to obtain a relief layer. After natural drying, the surface of the relief layer is covered with a 0.25 mm thick copper sheet to obtain a copper relief.
[0086] Comparative Example 1
[0087] A copper relief processing technology comprises the following steps:
[0088] S1, dissolving 10g of carboxymethyl chitosan in 100g of deionized water, then adding 4g of guanidine sulfamate and 5g of epichlorohydrin thereto, stirring and reacting at 50°C for 5h, after the reaction is completed, cooling to room temperature, then adding 20g of 10wt% sodium polyphosphate solution, stirring for 30min, to obtain an adhesive;
[0089] S2. Use a glue coating machine to evenly roll the prepared adhesive onto the surface of the substrate layer. The selected substrate layer is eucalyptus board, and the coating amount of the adhesive is 150g / m 2 ;
[0090] S3, 10 parts of acrylic resin, 5 parts of sodium silicate solution, 1 part of sodium carboxymethyl cellulose, 0.2 parts of defoaming agent and 0.5 parts of dispersant are added to a container, stirred and mixed evenly to obtain a slurry, and then the slurry is poured into a kneader, and 20 parts of calcium carbonate, 10 parts of talc and 15 parts of aluminum hydroxide powder are poured into the kneader, kneaded for 5 minutes, and a soft mud material is obtained;
[0091] S4. Use a flat roller to roll the soft mud into a relief layer film with a thickness of 5 mm, and spread it flat on the bonding layer. Then use a three-dimensional pattern mold roller to roll the surface of the relief layer film to form a three-dimensional pattern to obtain a relief layer. After natural drying, cover the surface of the relief layer with a 0.1 mm thick copper sheet to obtain a copper relief.
[0092] Compared with Example 1, in Comparative Example 1, no zinc nitrate solution was added during the preparation of the adhesive.
[0093] Comparative Example 2
[0094] A copper relief processing technology comprises the following steps:
[0095] S1, dissolving 10g of carboxymethyl chitosan in 100g of deionized water, then adding 4g of guanidine sulfamate and 5g of epichlorohydrin thereto, stirring and reacting at 50°C for 5h, after the reaction is completed, cooling to room temperature, then adding 10g, 5wt% zinc nitrate solution, and continuing stirring for 1h to obtain an adhesive;
[0096] S2. Use a glue coating machine to evenly roll the prepared adhesive onto the surface of the substrate layer. The selected substrate layer is eucalyptus board, and the coating amount of the adhesive is 150g / m 2 ;
[0097] S3, 10 parts of acrylic resin, 5 parts of sodium silicate solution, 1 part of sodium carboxymethyl cellulose, 0.2 parts of defoaming agent and 0.5 parts of dispersant are added to a container, stirred and mixed evenly to obtain a slurry, and then the slurry is poured into a kneader, and 20 parts of calcium carbonate, 10 parts of talc and 15 parts of aluminum hydroxide powder are poured into the kneader, kneaded for 5 minutes, and a soft mud material is obtained;
[0098] S4. Use a flat roller to roll the soft mud into a relief layer film with a thickness of 5 mm, and spread it flat on the bonding layer. Then use a three-dimensional pattern mold roller to roll the surface of the relief layer film to form a three-dimensional pattern to obtain a relief layer. After natural drying, cover the surface of the relief layer with a 0.1 mm thick copper sheet to obtain a copper relief.
[0099] Compared with Example 1, in Comparative Example 2, no sodium polyphosphate solution was added during the preparation of the adhesive.
[0100] In order to test the performance of the adhesives prepared in Examples 1-4 and Comparative Examples 1-2, the adhesives prepared in Examples 1-4 and Comparative Examples 1-2 were coated on the first and second layers of three-layer eucalyptus plywood, with a coating amount of 150 g / m 2 The veneers are laid according to the principle that the textures of adjacent veneers are perpendicular to each other, and then the assembled plywood is put into the hot press for hot pressing. The hot pressing conditions are: hot pressing temperature is 120℃, pressure is 1.2MPa, hot pressing time is 10min, followed by cold pressing at a pressure of 1MPa for 0.5h, and then placed at room temperature for 24h to obtain the plywood.
[0101] Ten plywood specimens were sawn from each plywood sheet. The specimen size was: 50 mm long × 50 mm wide × 17 mm thick. They were divided into two groups. One group was placed at room temperature to measure its bonding strength. The tensile speed was 10 mm / min. The other group was placed in water at a temperature of 63°C for 3 hours, taken out and cooled at room temperature for 10 minutes, and then its bonding strength was measured. The test was carried out according to the national standard GB / T 17657-2013 test method. The tensile speed was 10 mm / min. The test results were averaged.
[0102] Limiting oxygen index: tested according to GB / T 2406.2-2009 standard;
[0103] The test results are shown in the following table:
[0104]
[0105] It can be seen from the table that the adhesive prepared by the present invention has good dry bonding strength, and at the same time has good water resistance and flame retardancy. When it is used for bonding relief plates, the overall structure of the product is firm and not easy to deform.
[0106] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modification or improvement made without departing from the spirit of the present invention belongs to the scope of protection claimed in the present invention.
Claims
1. A copper relief, the copper relief comprising a substrate layer, an adhesive layer and a relief layer, the surface of the relief layer being covered with a layer of copper skin, characterized in that: The relief layer comprises the following raw materials in parts by weight: 10-20 parts of acrylic resin, 5-10 parts of sodium silicate solution, 20-30 parts of calcium carbonate, 10-20 parts of talc, 15-25 parts of aluminum hydroxide powder, 1-3 parts of sodium carboxymethyl cellulose, 0.2-0.4 parts of defoaming agent, and 0.5-1 parts of dispersant; The bonding layer is an adhesive layer, and the preparation method of the adhesive is as follows: dissolving carboxymethyl chitosan in deionized water, then adding guanidine sulfamate and epichlorohydrin thereto, stirring to react, and after the reaction is completed, cooling to room temperature, then adding sodium polyphosphate solution, stirring for 30-60 minutes, and then adding zinc salt solution, and continuing to stir for 1-2 hours to obtain the adhesive.
2. The copper relief according to claim 1, characterized in that: The mass ratio of the carboxymethyl chitosan, deionized water, guanidine sulfamate, epichlorohydrin, sodium polyphosphate solution and zinc salt solution is 8-12:100-150:4-6:5-8:20-30:10-20.
3. The copper relief according to claim 1, characterized in that: The mass fraction of the sodium polyphosphate solution is 10-20%.
4. The copper relief according to claim 1, characterized in that: The mass fraction of the zinc salt solution is 5-10%.
5. The copper relief according to claim 1, characterized in that: The stirring reaction temperature is 50-80°C, and the stirring reaction time is 3-5h.
6. The copper relief according to claim 1, characterized in that: The mass fraction of the sodium silicate solution is 10-20%.
7. A copper relief processing technology as claimed in any one of claims 1 to 6, characterized in that: The steps include: S1. Evenly coating the prepared adhesive on the surface of the substrate layer to obtain an adhesive layer; S2, adding acrylic resin, sodium silicate solution, sodium carboxymethyl cellulose, defoamer and dispersant into a container by weight, stirring and mixing evenly to obtain slurry, then pouring the slurry into a kneader, and pouring calcium carbonate, talcum powder and aluminum hydroxide powder into the kneader, kneading for 3-5 minutes to obtain a soft mud material; S3, rolling the soft mud material into a relief layer film with a thickness of 1-10mm, and spreading it on the bonding layer, then rolling the surface of the relief layer film with a three-dimensional pattern mold roller to form a three-dimensional pattern to obtain a relief layer, and after drying, a layer of red copper skin is covered on the surface of the relief layer to obtain a copper relief.
8. The processing technology according to claim 7, characterized in that: In step S1, the coating amount of the adhesive is 150-200 g / m 2 .
9. The processing technology according to claim 7, characterized in that: In step S3, the thickness of the copper skin is 0.1-0.3 mm.
10. The processing technology according to claim 7, characterized in that: The method also includes polishing the surface of the copper relief. The selected polishing agent includes the following raw materials: 80-100 parts of hydrogen peroxide, 30-40 parts of sodium phosphate, 10-15 parts of disodium ethylenediaminetetraacetate, 10-15 parts of 5-aminosalicylic acid, 3-5 parts of nano silicon dioxide, 8-10 parts of alkylphenol polyoxyethylene ether, and 5-10 parts of sodium lignin sulfonate.