Preparation method of nonmetal-doped layered porous carbon material

Through hydrothermal treatment and high-temperature activation methods, waste biomass is converted into non-metal doped porous carbon materials, solving the problems of insufficient conductivity and electrochemical performance of layered porous carbon materials, and achieving super-high energy density and cyclic stability Capacitor material preparation simplifies the process and reduces costs.

CN119018892AInactive Publication Date: 2024-11-26JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411267762.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing layered porous carbon materials have low specific surface area, uneven pore size distribution, low conductivity and electrochemical properties during the preparation process, which limits their application in electrode materials and supercapacitors.

Method used

Using a combination of hydrothermal treatment and high-temperature activation, waste biomass is converted into a non-metal doped porous carbon electrode material, hydrothermal reaction is carried out by a mixed solution of deionized water and ethanol, and high temperature is carried out under nitrogen or argon atmosphere. Activation, non-metal dopants are introduced to improve the surfactivity and conductivity of the material.

Benefits of technology

It significantly improves the energy density and cycle stability of supercapacitors, simplifies the preparation process, reduces costs, is suitable for industrial mass production, and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018892A_ABST
    Figure CN119018892A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a nonmetal doped layered porous carbon material, and belongs to the technical field of electrode materials.The method comprises the two steps that firstly, a biomass raw material is carbonized through a hydrothermal method, so that a carbon-based structure is formed preliminarily; then, a small amount of non-metal ions are introduced while high-temperature activation is carried out, the pore structure and the surface property of the material are further optimized, and therefore the high-performance electrode material is obtained. The prepared biomass carbon material has extremely high specific surface area and specific capacitance, and shows a highly regular porous morphology. According to the structural design, the transmission of electrolyte ions is effectively promoted, and the internal resistance of the material is reduced, so that the overall electrochemical performance of the supercapacitor is improved. When the material is simultaneously applied to positive and negative electrode materials of a symmetric supercapacitor, the device shows excellent cycling stability and relatively high energy density. The method disclosed by the invention has the characteristics of simplicity and convenience in operation and low cost, and industrial batch production is easy to realize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0002] The invention relates to the technical field of electrode materials, and in particular to a method for preparing a non-metal-doped layered porous carbon material. Background Art

[0003] As a commonly used electrode material for supercapacitors, hierarchical porous carbon materials have attracted great attention and research due to their excellent properties such as good cycle stability, low cost, non-toxicity, and environmental friendliness. However, during the preparation process, they have low specific surface area, uneven pore size distribution, low conductivity and electrochemical performance, which limits their application in electrode materials and supercapacitors.

[0004] There are many common ways to prepare hierarchical porous carbon materials, such as hydrothermal method, solvothermal method, calcination method, microwave method, template method, etc. In contrast, we proposed a method to enhance the specific surface area, conductivity and electrochemical properties of biomass carbon materials by doping non-metallic elements (such as boron, nitrogen, fluorine, sulfur, phosphorus, etc.). Doping with non-metallic elements can effectively adjust the electronic structure of carbon materials by introducing non-metallic functional groups, improve their surface activity and conductivity, and thus improve the specific capacitance and energy density of supercapacitors. However, how to achieve uniform doping of non-metallic elements through a simple and low-cost method, and maintain the porous structure of the material while ensuring high conductivity, is still a difficult problem in current research. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a method for preparing non-metal doped layered porous carbon materials. By combining hydrothermal treatment and high-temperature activation, waste biomass is converted into non-metal doped porous carbon electrode materials, and they are used as positive and negative electrode materials of supercapacitors.

[0006] In order to achieve the purpose of the above invention, the present invention provides the following technical solutions: The present invention provides a method for preparing a non-metal-doped layered porous carbon material, the method comprising the following steps: (1) The selected biomass material is washed, then dried at a temperature of 60 to 180 °C, and then shredded into small pieces with a particle size of 1 to 5 mm for subsequent processing; (2) using a mixed solution of deionized water and ethanol as a medium for hydrothermal reaction, and putting it into a reactor at a mass ratio of biomass material to reaction medium of 1:(2-20), and subjecting the treated biomass material to hydrothermal reaction at a temperature of 100-300°C for a reaction time of 12-36 hours; after the reaction is completed, removing impurities by centrifugation and washing with water, and drying to obtain a precursor; the volume fraction of ethanol in the mixed solution of deionized water and ethanol is 1%-99%; (3) The precursor is mixed with potassium hydroxide and a non-metallic dopant in a mass ratio of 1:(2-6):(0.2-2), placed in a tube furnace, and heated at 2-10 °C min in a nitrogen (N2) or argon (Ar) atmosphere. -1 The temperature is raised to 600-1200°C at a heating rate of 0.5-4 hours for activation; the activation time is 0.5-4 hours; then, the obtained product is acid-washed and water-washed in sequence to remove residual impurities, and then dried to obtain the non-metal-doped layered porous carbon material; Among them, the non-metallic dopant is a combination of one or more of a nitrogen source, a phosphorus source, a sulfur source, a boron source, and a halogen source; the nitrogen source is a combination of one or more of C3N4, NH4NO3, NH4HCO3 and melamine; the phosphorus source is a combination of one or more of H3PO4 and Na3PO4; the sulfur source is a combination of one or more of Na2S, sulfur powder and thiourea; the boron source is a combination of one or more of H3BO3, Zn3B2O6 and Na3BO3; the halogen source is a combination of one or more of NH4Cl, NH4F, NaF and KCl.

[0007] The biomass material in step (1) is various waste biomass, preferably a combination of one or more of fruit peels (orange peels, melon peels, banana peels), coconut shells, corn cobs, and bamboo scraps; Preferably, the cleaning method in step (1) is water cleaning, ethanol cleaning or ultrasonic cleaning in water; Preferably, during the centrifugal separation in step (2), the centrifugal speed is set to 5000-12000 rpm, and the centrifugal time is set to 3-15 minutes; Preferably, dilute hydrochloric acid, dilute sulfuric acid or dilute nitric acid is used for pickling in step (3); The non-metal-doped layered porous carbon material provided by the present invention can be used as positive and negative electrodes to assemble into a symmetrical supercapacitor in an aqueous electrolyte. The specific method is: (1) adding the non-metal-doped hierarchical porous carbon material, the conductive agent, and the binder in a mass ratio of (7-9):(0.5-1.5):(0.5-1.5) to anhydrous ethanol in sequence, and then heating and stirring at 80-90° C. until the anhydrous ethanol is evaporated, and then adding a small amount of ethanol to the dried powder to moisten the powder, rolling it into a thin sheet and drying it to obtain a carbon sheet; (2) According to the required size of the electrode, a current collector of corresponding size is taken, the carbon sheet prepared in step (4) is cut, and the carbon sheet is pressed onto the current collector to obtain the positive and negative electrodes of the supercapacitor.

[0008] Preferably, the conductive agent in step (1) is one of acetylene black, Ketjen black and carbon black; Preferably, the binder in step (1) may be one of polytetrafluoroethylene and polyvinylidene fluoride; Preferably, the electrolyte in step (1) can be one of sulfuric acid, sodium sulfate and potassium hydroxide; Preferably, the current collector in step (1) can be one of processed nickel foam, stainless steel, and carbon paper; Preferably, in step (2), the pressure at which the carbon sheet is pressed onto the current collector is controlled between 4 and 20 MPa.

[0009] Beneficial effects of the present invention: 1. The hydrothermal reaction and high-temperature activation process used simplifies the preparation process of carbon materials, avoids the complex chemical reagents and complex operations in traditional methods, and thus significantly improves the convenience of operation. By introducing non-metallic dopants, the present invention can efficiently incorporate non-metallic elements, enhance the surface activity and specific surface area of ​​carbon materials, and thus significantly improve the energy density and cycle stability of supercapacitors. The prepared carbon material exhibits excellent specific surface area and electrochemical properties, and exhibits good conductivity and high specific capacity (323.5 F g -1 ), making the assembled supercapacitor have an energy density (31.8Wh Kg -1 ) and power density.

[0010] 2. This method is simple to operate, low-cost, and suitable for industrial mass production. Using waste biomass materials as raw materials not only effectively reduces production costs, but also meets environmental protection requirements and sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a flow chart for the specific implementation of the method of the present invention; Figure 2 The SEM images of the non-metal-doped layered porous carbon material of the present invention at different activator ratios; Figure 3 Physical characterization diagrams of the non-metal-doped hierarchical porous carbon materials of the present invention: (a) contact angle test diagrams of different embodiments, (b) nitrogen adsorption-desorption curves of different embodiments; Figure 4 The performance test results of the non-metal-doped layered porous carbon material of the present invention are as follows: (a) cyclic voltammetry curves of Example 1 at different scanning speeds, (b) constant current charge-discharge curves of Example 1 at different current densities, (c) impedance spectrum of Example 1; Figure 5 : is the cycle stability curve of the symmetrical supercapacitor assembled in Example 1. DETAILED DESCRIPTION

[0012] The method for preparing the non-metal-doped layered porous carbon material provided by the present invention is described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0013] Example 1 (KPC-SP-1) (1) Weigh 10 g of Hami melon rind, wash it with water, and dry it in a vacuum oven at 100 °C for 18 h. Cut the dried Hami melon rind into pieces with a particle size of about 2 mm.

[0014] (2) A mixed solution of deionized water and ethanol was used as the medium for the hydrothermal reaction, with the volume fraction of ethanol being 50%. Hami melon peel was placed in a reactor at a mass ratio of 1:10, and the hydrothermal reaction was carried out at 200 °C for 24 hours. The cooled product was centrifuged at 8000 rpm for 5 minutes, and the washed material was dried in a vacuum oven at 100 °C for 18 hours.

[0015] (3) The pretreated precursor was mixed with KOH at a mass ratio of 1:4, and the non-metallic dopants were thiourea and sodium hypophosphite, which were 1 times the mass of the precursor. The activation temperature was set at 900 °C, and the activation was carried out in a nitrogen atmosphere with a heating rate of 5 °C min -1 The reaction time was 2 hours. The cooled product was washed with hydrochloric acid and the washed material was dried in a vacuum oven at 100°C for 18 hours.

[0016] (4) The prepared layered porous carbon, acetylene black, and polytetrafluoroethylene were uniformly mixed in a mass ratio of 8:1:1, and the treated nickel foam was selected as the current collector. The pressing pressure was controlled at 8 MPa, and the electrolyte was sodium sulfate. A symmetrical supercapacitor was assembled.

[0017] Example 2 (1) Weigh 10 g of kiwifruit peel, wash it with water, and dry it in a vacuum oven at 100 °C for 18 h. After drying, cut the kiwifruit peel into pieces with a particle size of about 2 mm.

[0018] (2) A mixed solution of deionized water and ethanol was used as the medium for the hydrothermal reaction. The volume fraction of ethanol was 50%. The kiwifruit peel was placed in a reactor at a mass ratio of 1:10 and the hydrothermal reaction was carried out at 200 °C for 24 hours. The cooled product was centrifuged at 8000 rpm for 5 minutes, and the washed material was dried in a vacuum oven at 100 °C for 18 hours.

[0019] (3) The pretreated precursor was mixed with KOH at a mass ratio of 1:4, and the non-metallic dopants were thiourea and sodium hypophosphite, which were 1 times the mass of the precursor. The activation temperature was set at 900 °C, and the activation was carried out in a nitrogen atmosphere with a heating rate of 5 °C min -1 The reaction time was 2 hours. The cooled product was washed with hydrochloric acid and the washed material was dried in a vacuum oven at 100°C for 18 hours.

[0020] (4) The prepared layered porous carbon, acetylene black, and polytetrafluoroethylene were uniformly mixed in a mass ratio of 8:1:1, and the treated nickel foam was selected as the current collector. The pressing pressure was controlled at 8 MPa, and the electrolyte was sodium sulfate. A symmetrical supercapacitor was assembled.

[0021] Example 3 (KPC-SP-0.5) (1) Weigh 10 g of Hami melon rind, wash it with water, and dry it in a vacuum oven at 100 °C for 18 h. Cut the dried Hami melon rind into pieces with a particle size of about 2 mm.

[0022] (2) A mixed solution of deionized water and ethanol was used as the medium for the hydrothermal reaction, with the volume fraction of ethanol being 50%. Hami melon peel was placed in a reactor at a mass ratio of 1:10, and the hydrothermal reaction was carried out at 200 °C for 24 hours. The cooled product was centrifuged at 8000 rpm for 5 minutes, and the washed material was dried in a vacuum oven at 100 °C for 18 hours.

[0023] (3) The pretreated precursor was mixed with KOH at a mass ratio of 1:3. The non-metallic dopants were thiourea and sodium hypophosphite, which were 0.5 times the mass of the precursor. The activation temperature was set at 900 °C and the activation was carried out in a nitrogen atmosphere with a heating rate of 5 °C min -1 The reaction time was 2 hours. The cooled product was washed with hydrochloric acid and the washed material was dried in a vacuum oven at 100°C for 18 hours.

[0024] (4) The prepared layered porous carbon, acetylene black, and polytetrafluoroethylene were uniformly mixed in a mass ratio of 8:1:1, and the treated nickel foam was selected as the current collector. The pressing pressure was controlled at 8 MPa, and the electrolyte was sodium sulfate. A symmetrical supercapacitor was assembled.

[0025] Example 4 (KPC-SP-2) (1) Weigh 10 g of Hami melon rind, wash it with water, and dry it in a vacuum oven at 100 °C for 18 h. Cut the dried Hami melon rind into pieces with a particle size of about 2 mm.

[0026] (2) A mixed solution of deionized water and ethanol was used as the medium for the hydrothermal reaction, with the volume fraction of ethanol being 50%. Hami melon peel was placed in a reactor at a mass ratio of 1:10, and the hydrothermal reaction was carried out at 200 °C for 24 hours. The cooled product was centrifuged at 8000 rpm for 5 minutes, and the washed material was dried in a vacuum oven at 100 °C for 18 hours.

[0027] (3) The pretreated precursor was mixed with KOH at a mass ratio of 1:3. The non-metallic dopants were thiourea and sodium hypophosphite, which were twice the mass of the precursor. The activation temperature was set at 900 °C and the activation was carried out in a nitrogen atmosphere with a heating rate of 5 °C min -1 The reaction time was 2 hours. The cooled product was washed with hydrochloric acid and the washed material was dried in a vacuum oven at 100°C for 18 hours.

[0028] (4) The prepared layered porous carbon, acetylene black, and polytetrafluoroethylene were uniformly mixed in a mass ratio of 8:1:1, and the treated nickel foam was selected as the current collector. The pressing pressure was controlled at 8 MPa, and the electrolyte was sodium sulfate. A symmetrical supercapacitor was assembled.

[0029] Comparative Example 1 (Tested in the same manner without introducing heteroatom dopants) (1) Weigh 10 g of Hami melon rind, wash it with water, and dry it in a vacuum oven at 100 °C for 18 h. Cut the dried Hami melon rind into pieces with a particle size of about 2 mm.

[0030] (2) A mixed solution of deionized water and ethanol was used as the medium for the hydrothermal reaction, with the volume fraction of ethanol being 50%. Hami melon peel was placed in a reactor at a mass ratio of 1:10, and the hydrothermal reaction was carried out at 200 °C for 24 hours. The cooled product was centrifuged at 8000 rpm for 5 minutes, and the washed material was dried in a vacuum oven at 100 °C for 18 hours.

[0031] (3) The pretreated precursor was mixed with KOH at a mass ratio of 1:4, and the activation temperature was set at 900 °C. The activation was carried out in a nitrogen atmosphere at a heating rate of 5 °C min -1 The reaction time was 2 hours. The cooled product was washed with hydrochloric acid and the washed material was dried in a vacuum oven at 100°C for 18 hours.

[0032] (4) The prepared layered porous carbon, acetylene black, and polytetrafluoroethylene were uniformly mixed in a mass ratio of 8:1:1, and the treated nickel foam was selected as the current collector. The pressing pressure was controlled at 8 MPa, and the electrolyte was sodium sulfate. A symmetrical supercapacitor was assembled.

[0033] Comparative Example 2 (Tested in the same way without hydrothermal operation, (KPC-1:4)) (1) Weigh 10 g of Hami melon rind, wash it with water, and dry it in a vacuum oven at 100 °C for 18 h. Cut the dried Hami melon rind into pieces with a particle size of about 2 mm.

[0034] (2) Chopped cantaloupe peel was mixed with KOH in a mass ratio of 1:4. Thiourea and sodium hypophosphite were selected as non-metallic dopants, which were 1 times the mass of the precursor. The activation temperature was set at 900 °C and the activation was carried out in a nitrogen atmosphere with a heating rate of 5 °C min -1 The reaction time was 2 hours. The cooled product was washed with hydrochloric acid and the washed material was dried in a vacuum oven at 100°C for 18 hours.

[0035] (3) The prepared layered porous carbon, acetylene black, and polytetrafluoroethylene were uniformly mixed in a mass ratio of 8:1:1, and the treated nickel foam was selected as the current collector. The pressing pressure was controlled at 8 MPa, and the electrolyte was sodium sulfate. A symmetrical supercapacitor was assembled.

[0036] The SEM images of the non-metal-doped hierarchical porous carbon material prepared by the hydrothermal and activation method provided by the present invention are as follows: Figure 2 shown.

[0037] Performance Testing The materials obtained in Example 1, Example 2, Example 3, and Comparative Example 1 and Comparative Example 2 were used as positive and negative electrode materials of symmetrical supercapacitors, and their specific capacitance was tested in 6 M KOH solution under a three-electrode system. A symmetrical supercapacitor was formed, and the electrochemical performance was tested in 1 M Na2SO4 solution to obtain the energy density under the system. The results are shown in Table 1.

[0038] Table 1 Test results of specific capacitance and energy density in the examples and comparative examples <![CDATA[Specific capacitance F g -1 > <![CDATA[Energy density Wh Kg -1 > Example 1 323.5 31.8 Example 2 (Replacing biomass materials) 313.8 30.5 Example 3 (changing the doping amount to 0.5) 302.1 29.7 Example 4 (changing the doping amount to 2) 294.4 29.1 Comparative Example 1 (without adding non-metallic dopant) 269.0 27.4 Comparative Example 2 (no hydrothermal treatment, direct activation) 207.5 20.3 (1) From Table 1 and Figure 2~Figure 5 It can be seen that by using different biomass, the performance of the prepared hierarchical porous carbon materials is roughly similar, and they have rich macropores, mesopores, and micropore structures, and have high disorder. In addition, with the increase of the doping amount, the hydrophilicity, specific surface area, specific capacitance of the carbon material and the energy density of the assembled symmetric supercapacitor show a trend of first increasing and then decreasing, reaching the maximum value when the doping ratio is 1:1. In addition, it also has good stability, with a stability of 92.17% after 25,000 cycles.

[0039] (2) By testing the electrochemical properties of Example 1 and Comparative Example 1, it can be found that without adding non-metallic dopants, the energy density and specific capacitance both decrease.

[0040] (3) Through the electrochemical performance test of Example 1 and Comparative Example 2, it can be found that without hydrothermal carbonization, the energy density and specific capacitance are both reduced.

[0041] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a non-metal-doped layered porous carbon material, characterized in that: The method comprises the following steps: (1) The selected biomass material is washed, then dried at a temperature of 60 to 180 °C, and then shredded into small pieces with a particle size of 1 to 5 mm for subsequent processing; (2) using a mixed solution of deionized water and ethanol as a medium for hydrothermal reaction, and putting it into a reactor at a mass ratio of biomass material to reaction medium of 1:(2-20), and subjecting the treated biomass material to hydrothermal reaction at a temperature of 100-300°C for a reaction time of 12-36 hours; after the reaction is completed, removing impurities by centrifugation and washing with water, and drying to obtain a precursor; the volume fraction of ethanol in the mixed solution of deionized water and ethanol is 1%-99%; (3) The precursor is mixed with potassium hydroxide and a non-metallic dopant in a mass ratio of 1:(2-6):(0.2-2), placed in a tube furnace, and heated at 2-10 °C min-1 in a nitrogen or argon atmosphere. -1 The temperature is raised to 600-1200°C at a heating rate of 0.5-4 hours for activation; the activation time is 0.5-4 hours; then, the obtained product is acid-washed and water-washed in sequence to remove residual impurities, and then dried to obtain the non-metal-doped layered porous carbon material; Among them, the non-metallic dopant is a combination of one or more of a nitrogen source, a phosphorus source, a sulfur source, a boron source, and a halogen source; the nitrogen source is a combination of one or more of C3N4, NH4NO3, NH4HCO3 and melamine; the phosphorus source is a combination of one or more of H3PO4 and Na3PO4; the sulfur source is a combination of one or more of Na2S, sulfur powder and thiourea; the boron source is a combination of one or more of H3BO3, Zn3B2O6 and Na3BO3; the halogen source is a combination of one or more of NH4Cl, NH4F, NaF and KCl.

2. The method for preparing a non-metal-doped layered porous carbon material according to claim 1, characterized in that: The biomass material in step (1) is selected from various waste biomasses.

3. The non-metal-doped layered porous carbon material prepared according to the method of claim 1 or 2.

4. Use of the non-metal-doped layered porous carbon material as claimed in claim 3 as positive and negative electrodes in an aqueous electrolyte to assemble into a symmetrical supercapacitor.

5. Use of non-metal-doped hierarchical porous carbon material according to claim 4, characterized in that: The steps for preparing the positive and negative electrodes of the supercapacitor are as follows: (1) adding the non-metal-doped hierarchical porous carbon material, the conductive agent, and the binder in a mass ratio of (7-9):(0.5-1.5):(0.5-1.5) to anhydrous ethanol in sequence, and then heating and stirring at 80-90° C. until the anhydrous ethanol is evaporated, and then adding a small amount of ethanol to the dried powder to moisten the powder, rolling it into a thin sheet and drying it to obtain a carbon sheet; (2) According to the required size of the electrode, a current collector of corresponding size is taken, the carbon sheet prepared in step (4) is cut, and the carbon sheet is pressed onto the current collector to obtain the positive and negative electrodes of the supercapacitor.

6. Use of non-metal-doped hierarchical porous carbon material according to claim 5, characterized in that: The conductive agent in step (1) is one of acetylene black, Ketjen black and carbon black.

7. The use of non-metal-doped hierarchical porous carbon material according to claim 5, characterized in that: The binder in step (1) is one of polytetrafluoroethylene and polyvinylidene fluoride.

8. The use of non-metal-doped hierarchical porous carbon material according to claim 5, characterized in that: The electrolyte in step (1) is one of sulfuric acid, sodium sulfate and potassium hydroxide.

9. The use of non-metal-doped hierarchical porous carbon material according to claim 5, characterized in that: The current collector in step (1) is one of processed nickel foam, stainless steel and carbon paper.

10. The use of non-metal-doped hierarchical porous carbon material according to claim 5, characterized in that: In step (2), the pressure of the carbon sheet pressed on the current collector is controlled between 4 and 20 MPa.