Modification method of hydrophobic prussian blue positive electrode material, modified hydrophobic prussian blue positive electrode material, positive plate thereof and sodium ion battery
Through high-temperature baking and modified wrapping liquid treatment, a modified Prussian blue positive electrode material formed with a hydrophobic coating layer is solved, which solves the structural collapse problem caused by water absorption of Prussian blue materials and improves the circulation performance and production efficiency of sodium ion batteries.
Patent Information
- Application Number
- CN202411138079.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
The existing Prussian blue positive electrode materials are prone to absorb water during charging and discharging, causing structural collapse, affecting the circulation stability of sodium ion batteries. In addition, the early low-surface energy modifiers have odor and poor oxidation, resulting in a short battery cycle life.
After high-temperature baking, the oxysilane coupling agent, organic solvent and a small amount of deionized water are mixed to form a modified wrapping liquid, and the oxysilane coupling agent is filled with holes in the Prussian blue positive electrode material through ultrasonic and water bath heating. A hydrophobic coating is formed to improve its hydrophobicity and lipophilicity.
The high hydrophobicity and lipophilicity of the modified Prussian blue cathode material are achieved, the adhesion between the cathode slurry and the current collector is enhanced, the circulation performance of the sodium ion battery is improved, the preparation time is shortened, and the production efficiency is improved.
Smart Images

Figure CN119018910A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a method for modifying a hydrophobic Prussian blue positive electrode material, a modified hydrophobic Prussian blue positive electrode material and a positive electrode sheet thereof, and a sodium ion battery. Background Art
[0002] In recent years, the cost of lithium-ion batteries has increased significantly, and low-cost sodium-ion batteries have become more advantageous in comparison. Because sodium ore resources are vast, cost-effective, and volatile, it is expected to replace lead-acid batteries or lithium iron phosphate batteries in the energy storage market in the future.
[0003] Sodium ion positive electrode material is one of the main raw materials for sodium ion batteries. It is mainly divided into three categories: Prussian blue series, layered oxide series, polyanion and its derivative series. Due to the advantages of low cost, high specific capacity, high energy density and simple synthesis, the Prussian blue series has great industrial prospects. The Prussian blue series is mainly based on Prussian blue materials. However, since the Prussian blue material contains a certain proportion of crystal water and is very easy to absorb water during the production process, the final prepared Prussian blue material positive electrode material is prone to structural collapse during the charge and discharge process, which affects the stability of the sodium battery cycle.
[0004] In order to solve the above technical problems, the market has adopted the method of coating and modifying the positive electrode material of Prussian blue material with a low specific surface energy modifier to inhibit the water absorption of the positive electrode material of Prussian blue material. The early low surface energy modifiers generally used thiol surface modifiers, but because thiol surface modifiers have a strong odor and are highly irritating to the human body, and thiol has poor antioxidant capacity, it is easily oxidized during the charge and discharge process, resulting in a short cycle life of the sodium ion battery.
[0005] For this reason, a new method for modifying the positive electrode material of Prussian blue material has appeared on the market. As Chinese patent document CN 116040654 A discloses a super-hydrophobic Prussian blue material and its preparation method and application, by adding a fluorosilane coupling agent to the positive electrode material of the Prussian blue material, the fluorosilane coupling agent can form a super-hydrophobic layer on the surface of the positive electrode material of the Prussian blue material, thereby effectively improving the cycle performance of the sodium ion battery and reducing the irritation to the human body.
[0006] Although the fluorosilane coupling agent used in the above-mentioned Prussian blue material positive electrode material modification method can form an extremely low low surface hydrophobic layer on the surface of the Prussian blue material positive electrode material, that is, the hydrophobicity of the Prussian blue material positive electrode material is greatly improved. However, since the low surface hydrophobic layer formed by the above-mentioned Prussian blue material positive electrode material will weaken its oleophilic properties, its compatibility and dispersibility in the positive electrode slurry will deteriorate, that is, the adhesion between the Prussian blue material positive electrode material and the positive electrode binder PVDF is reduced, resulting in low adhesion between the positive electrode slurry and the current collector, which affects the cycle performance of the sodium ion battery. Summary of the invention
[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a modified hydrophobic Prussian blue positive electrode material with extremely low moisture content, good lipophilicity and hydrophobicity, and high connection strength, which not only improves the adhesion between the positive electrode slurry and the current collector, but also shortens the baking time of the positive electrode sheet, a modified hydrophobic Prussian blue positive electrode material, a positive electrode sheet thereof, and a sodium ion battery.
[0008] The purpose of this disclosure is achieved through the following technical solutions:
[0009] A method for modifying a hydrophobic Prussian blue cathode material.
[0010] Obtain Prussian blue cathode material;
[0011] Performing a high temperature baking operation on the Prussian blue positive electrode material;
[0012] The oxysilane coupling agent, the organic solvent and a small amount of deionized water are mixed to obtain a modified coating liquid;
[0013] Putting the Prussian blue positive electrode material after high temperature baking into the modified coating liquid to obtain a mixed liquid;
[0014] performing ultrasonic operation on the mixed solution;
[0015] Heating the mixed solution after ultrasonic operation in a water bath;
[0016] The mixed solution subjected to water bath heating operation is filtered to obtain filter residue;
[0017] The filter residue is dried to obtain a modified hydrophobic Prussian blue positive electrode material.
[0018] In one embodiment, the water contact angle of the modified hydrophobic Prussian blue positive electrode material is 100° to 130°.
[0019] In one embodiment, the organic solvent is one or more of methanol, ethanol, acetone, isopropanol, n-butanol, furan, chloroform, N-methylpyrrolidone, benzene, and dimethyl sulfoxide.
[0020] In one embodiment, the weight ratio of the oxysilane coupling agent to deionized water is (7-45): (0.5-1).
[0021] In one embodiment, the weight ratio of the Prussian blue positive electrode material to the oxysilane coupling agent is 100:(0.3-5).
[0022] In one embodiment, the oxysilane coupling agent includes at least one of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane.
[0023] In one embodiment, the conditions of the high temperature baking operation are: temperature 150° C. to 230° C.; time 5 h to 48 h; and / or,
[0024] The conditions of the water bath heating operation are: conducting a water bath in an inert atmosphere, controlling the water bath temperature to 45° C. to 90° C., the water bath time to 10 min to 120 min, and the pH to 5 to 8; and / or,
[0025] The weight ratio of the organic solvent to the oxysilane coupling agent is 1:(8-12).
[0026] A modified hydrophobic Prussian blue positive electrode material is prepared by using the modification method of the hydrophobic Prussian blue positive electrode material described in any one of the above embodiments.
[0027] A modified hydrophobic Prussian blue positive electrode sheet comprises a current collector and a positive electrode slurry coated on the current collector, wherein the positive electrode slurry comprises the modified hydrophobic Prussian blue positive electrode material described in any one of the above embodiments.
[0028] A sodium ion battery comprises the modified hydrophobic Prussian blue positive electrode sheet according to any one of the above embodiments.
[0029] Compared with the prior art, the present invention has at least the following advantages:
[0030] 1) Firstly, a Prussian blue cathode material is subjected to a high-temperature baking operation to effectively remove the crystal water in the Prussian blue cathode material to leave holes, and an oxysilane coupling agent, an organic solvent and a small amount of deionized water are mixed to obtain a modified coating liquid, so as to realize the separate preparation of the modified coating liquid, and effectively avoid the problem that deionized water is directly added to the Prussian blue cathode material after high-temperature baking and interferes with the oxysilane coupling agent filling the holes of the Prussian blue cathode material; then, the Prussian blue cathode material after high-temperature baking is placed in the modified coating liquid, and then an ultrasonic operation is performed, so that the oxysilane coupling agent in the modified coating liquid can be quickly and evenly dispersed on the surface of the Prussian blue cathode material, and as the ultrasonic operation is continuously performed, the oxysilane coupling agent in the modified coating liquid can be quickly and efficiently filled in the holes, so that the modified coating liquid can fully occupy the holes of the Prussian blue cathode material, which not only improves the hydrophobicity inside the Prussian blue cathode material, but also improves the modified The connection strength between the modified coating liquid and the Prussian blue positive electrode material is improved; then the mixed solution after the ultrasonic operation is heated in a water bath to ensure that the added oxysilane coupling agent can achieve comprehensive cross-linking with the Prussian blue positive electrode material under the condition of a water bath, so that a hydrophobic coating layer is embedded on the surface of the Prussian blue positive electrode material to form a hydrophobic coating layer, thereby ensuring that the modified Prussian blue positive electrode material has both good oleophilic and hydrophobic characteristics, so that the added modified coating liquid has the characteristics of coupling the Prussian blue positive electrode material and the positive electrode binder PVDF at the same time, so that the surface electronegative groups of the hydrophobic coating layer of the modified Prussian blue positive electrode material can produce hydrogen bonds with the fluorine atoms of the positive electrode binder PVDF, thereby improving the compatibility and dispersibility of the modified Prussian blue positive electrode material in the positive electrode slurry, thereby increasing the adhesion between the modified Prussian blue positive electrode material and the positive electrode binder PVDF, thereby improving the adhesion between the positive electrode slurry and the current collector, and thereby improving the cycle performance of the sodium ion battery.
[0031] 2) Since the oxysilane coupling agent of the modified coating liquid can be quickly and efficiently filled in the cavities, the baking time for preparing the modified hydrophobic Prussian blue positive electrode sheet is effectively shortened, thereby improving the production efficiency of the modified hydrophobic Prussian blue positive electrode sheet. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 The figure is a flow chart of a method for modifying a hydrophobic Prussian blue positive electrode material according to an embodiment of the present invention. DETAILED DESCRIPTION
[0034] In order to facilitate the understanding of the present disclosure, the present disclosure will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present disclosure are given in the drawings. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present disclosure more thoroughly and comprehensively understood.
[0035] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present disclosure. The terms used herein in the specification of the present disclosure are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0037] The present invention provides a method for modifying a hydrophobic Prussian blue positive electrode material, comprising the following steps: obtaining a Prussian blue positive electrode material; performing a high-temperature baking operation on the Prussian blue positive electrode material; performing a mixing operation on an oxysilane coupling agent, an organic solvent and a small amount of deionized water to obtain a modified coating liquid; placing the Prussian blue positive electrode material after the high-temperature baking into the modified coating liquid to obtain a mixed liquid; performing an ultrasonic operation on the mixed liquid; performing a water bath heating operation on the mixed liquid after the ultrasonic operation; performing suction filtration on the mixed liquid after the water bath heating operation to obtain a filter residue; and drying the filter residue to obtain a modified hydrophobic Prussian blue positive electrode material.
[0038] The above-mentioned method for modifying the hydrophobic Prussian blue positive electrode material first performs a high-temperature baking operation on the Prussian blue positive electrode material to effectively remove the crystal water in the Prussian blue positive electrode material and leave holes, and mixes the oxysilane coupling agent, the organic solvent and a small amount of deionized water to obtain a modified coating liquid, so as to realize the separate preparation of the modified coating liquid, and effectively avoid the problem that the deionized water is directly added to the Prussian blue positive electrode material after high-temperature baking and interferes with the oxysilane coupling agent filling the holes of the Prussian blue positive electrode material; then the Prussian blue positive electrode material after high-temperature baking is placed in the modified coating liquid, and then ultrasonic operation is performed, so that the oxysilane coupling agent in the modified coating liquid can be quickly and evenly dispersed on the surface of the Prussian blue positive electrode material, and as the ultrasonic operation is continuously performed, the oxysilane coupling agent in the modified coating liquid can be quickly and efficiently filled in the holes, so that the modified coating liquid can fully occupy the holes of the Prussian blue positive electrode material, which not only improves the hydrophobicity inside the Prussian blue positive electrode material The invention discloses a method for improving the performance of the modified coating liquid and the connection strength between the modified coating liquid and the Prussian blue positive electrode material; then the mixed liquid after the ultrasonic operation is heated in a water bath to ensure that the added oxysilane coupling agent can achieve comprehensive cross-linking with the Prussian blue positive electrode material under the condition of a water bath, so that a hydrophobic coating layer is embedded on the surface of the Prussian blue positive electrode material to form a hydrophobic coating layer, thereby ensuring that the modified Prussian blue positive electrode material has both good oleophilic and hydrophobic characteristics, so that the added modified coating liquid has the characteristics of coupling the Prussian blue positive electrode material and the positive electrode binder PVDF at the same time, so that the surface electronegative groups of the hydrophobic coating layer of the modified Prussian blue positive electrode material can produce hydrogen bonds with the fluorine atoms of the positive electrode binder PVDF, thereby improving the compatibility and dispersibility of the modified Prussian blue positive electrode material in the positive electrode slurry, thereby increasing the adhesion between the modified Prussian blue positive electrode material and the positive electrode binder PVDF, thereby improving the adhesion between the positive electrode slurry and the current collector, and thereby improving the cycle performance of the sodium ion battery. Furthermore, since the oxysilane coupling agent of the modified coating liquid can be quickly and efficiently filled in the cavities, the baking time for preparing the modified hydrophobic Prussian blue positive electrode sheet is effectively shortened, thereby improving the production efficiency of the modified hydrophobic Prussian blue positive electrode sheet.
[0039] See also Figure 1 In order to better understand the technical solution and beneficial effects of the present disclosure, the present disclosure is further described in detail below in conjunction with specific embodiments. The modification method of the hydrophobic Prussian blue positive electrode material of one embodiment includes some or all of the following steps:
[0040] S101. Obtain Prussian blue positive electrode material for backup.
[0041] S102, performing a high temperature baking operation on the Prussian blue positive electrode material.
[0042] It can be understood that, since the Prussian blue positive electrode material has strong water absorption, if the Prussian blue positive electrode material is not dehydrated, the electrical properties of the Prussian blue positive electrode material will be affected, resulting in the problem of structural collapse of the Prussian blue positive electrode material during multiple charge and discharge processes. Therefore, in the present disclosure, the Prussian blue positive electrode material is subjected to a high-temperature baking operation to effectively remove the crystal water in the Prussian blue positive electrode material, and to leave holes in the Prussian blue positive electrode material so that the oxysilane coupling agent of the subsequent modified coating liquid can be filled in the holes.
[0043] It can be understood that if the baking temperature is lower than 150 ° C or the baking time is lower than 5h, the crystal water inside the Prussian blue positive electrode material cannot be removed more comprehensively; if the baking temperature is higher than 230 ° C or the baking time is higher than 48h, it is easy to cause the Prussian blue positive electrode material to have cracks and other undesirable phenomena. Therefore, in the present disclosure, by controlling the conditions of the high temperature baking operation to be: temperature 150 ° C ~ 230 ° C; time 5h ~ 48h, the baking conditions are better controlled to ensure that the baking temperature and time are relatively suitable, so as to achieve the removal of all the crystal water in the Prussian blue positive electrode material, so as to ensure that more holes can be formed inside the Prussian blue positive electrode material, which is conducive to the filling of more modified coating liquid, not only more comprehensively improving the hydrophobic performance inside the Prussian blue positive electrode material, but also better improving the connection strength between the modified coating liquid and the Prussian blue positive electrode material; effectively avoiding the problem of easy detachment of the hydrophobic coating layer and the Prussian blue positive electrode material during multiple cycles.
[0044] S103, mixing an oxysilane coupling agent, an organic solvent and a small amount of deionized water to obtain a modified coating liquid.
[0045] It can be understood that, as mentioned in the background technology, the use of low specific surface energy modifiers to coat and modify Prussian blue positive electrode materials is the research direction of many scholars. However, in order to pursue the high hydrophobicity of Prussian blue positive electrode materials, many scholars have ignored the problem that the high hydrophobicity leads to the lower oleophilicity, which leads to the deterioration of the compatibility and dispersibility of Prussian blue positive electrode materials in the positive electrode slurry.
[0046] In order to find a method that has both good lipophilicity and hydrophilicity, in the present disclosure, an oxysilane coupling agent, an organic solvent and a small amount of deionized water are mixed to achieve the separate preparation of the modified coating liquid, which effectively avoids the problem that the deionized water is directly added to the Prussian blue positive electrode material after high-temperature baking and interferes with the oxysilane coupling agent filling the holes of the Prussian blue positive electrode material, so that the surface energy of the oxysilane coupling agent is relatively higher than that of the traditional fluorosilane coupling agent, so as to ensure that the modified coating liquid has the ability to couple the Prussian blue positive electrode material. The characteristics of the material and the positive electrode binder PVDF, that is, the oxysilane functional groups in the modified coating liquid can cross-link with the Prussian blue positive electrode material to be embedded in the holes and outer surface of the Prussian blue positive electrode material, and can also produce hydrogen bonds with the fluorine atoms of the positive electrode binder PVDF; thereby improving the compatibility and dispersibility of the modified Prussian blue positive electrode material in the positive electrode slurry, thereby increasing the adhesion between the modified Prussian blue positive electrode material and the positive electrode binder PVDF, thereby improving the adhesion between the positive electrode slurry and the current collector, and thereby improving the cycle performance of the sodium ion battery.
[0047] It should also be noted that in order to ensure that the oxysilane coupling agent can be well dispersed in the modified coating liquid, the oxysilane coupling agent, the organic solvent and a small amount of deionized water are mixed so that the oxysilane coupling agent can be well dispersed in the modified coating liquid, thereby obtaining a modified coating liquid with a stable dispersion system and uniformity.
[0048] It is worth mentioning that if deionized water is added directly into the Prussian blue positive electrode material, the Prussian blue positive electrode material will quickly absorb the deionized water and affect the filling of the oxysilane coupling agent in the modified coating liquid. Therefore, in the present disclosure, the oxysilane coupling agent, the organic solvent and a small amount of deionized water are mixed so that the oxysilane coupling agent can be fully mixed and dispersed with a small amount of deionized water, thereby obtaining a modified coating liquid with a stable and uniform dispersion system, effectively avoiding the problem of directly adding deionized water to affect the filling of the modified coating liquid. Adding a small amount of deionized water is beneficial to the subsequent ultrasonic operation of the modified coating liquid with the Prussian blue positive electrode material, so that the modified coating liquid can be quickly and efficiently filled in the holes. At the same time, accompanied by the water bath operation, the modified coating liquid is continuously hydrolyzed under high temperature conditions. In this way, the free water in the modified coating liquid can be fully consumed, and the surface energy of the modified coating liquid is also increased, so that the modified coating liquid can be more fully and comprehensively cross-linked in the holes of the Prussian blue positive electrode material. In this way, while the connection strength between the modified coating liquid and the Prussian blue positive electrode material is improved, the moisture content of the finally prepared hydrophobic coating layer is ensured to be extremely low, which better guarantees the electrical properties of the modified Prussian blue positive electrode material.
[0049] It can be understood that if the content of deionized water added is high, the modified coating liquid obtained by mixing will contain more free water. When the modified coating liquid is mixed with the Prussian blue positive electrode material, more free water will more easily occupy the vacant positions of the Prussian blue positive electrode material and interfere with the filling of the oxysilane coupling agent in the modified coating liquid. If the content of deionized water added is low, it cannot be guaranteed that the oxysilane coupling agent can achieve a good cross-linking effect with the Prussian blue positive electrode material during the subsequent water bath operation, resulting in the problem of poor connectivity between the modified coating liquid and the Prussian blue positive electrode material. Therefore, in one embodiment, the weight ratio of the oxysilane coupling agent to deionized water is (7-45): (0.5-1), so as to ensure that the addition of a small amount of deionized water can fully disperse the mixed oxysilane coupling agent, effectively avoiding the presence of more free water in the modified coating liquid and interfering with the filling of the oxysilane coupling agent in the modified coating liquid, so as to ensure the subsequent preparation of a modified hydrophobic Prussian blue positive electrode material with strong connectivity and good lipophilicity and hydrophobicity.
[0050] In one embodiment, the organic solvent is one or more of methanol, ethanol, acetone, isopropanol, n-butanol, furan, chloroform, N-methylpyrrolidone, benzene, and dimethyl sulfoxide.
[0051] In one embodiment, the weight ratio of the organic solvent to the oxysilane coupling agent is 1:(8-12). If too much organic solvent is added, the concentration of the oxysilane coupling agent will be low, resulting in a low crosslinking efficiency; if less organic solvent is added, the oxysilane coupling agent will be easily unevenly dispersed. Therefore, in the present disclosure, by controlling the weight ratio of the organic solvent to the oxysilane coupling agent to be 1:(8-12), the added organic solvent and deionized water can better disperse and mix the oxysilane coupling agent, while also better ensuring the efficiency of the crosslinking of the oxysilane coupling agent.
[0052] In one embodiment, the oxysilane coupling agent includes at least one of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane to ensure that the prepared modified coating liquid contains oxysilane functional groups, so that the oxysilane functional groups can simultaneously have the characteristics of coupling Prussian blue positive electrode material and positive electrode binder PVDF, so that the oxysilane functional groups can cross-link with the Prussian blue positive electrode material to be embedded in the cavities and outer surface of the Prussian blue positive electrode material, and the oxysilane functional groups can also produce hydrogen bonds with the fluorine atoms of the positive electrode binder PVDF, thereby improving the adhesion with the positive electrode binder PVDF.
[0053] In one embodiment, the oxysilane coupling agent is placed in an organic solvent, and then a small amount of deionized water is dropped into it and stirred evenly, so that the oxysilane coupling agent can be fully dispersed in the organic solvent and deionized water, and finally allowed to stand for 5 minutes to 15 minutes, thereby ensuring that a stable and uniform modified coating liquid is prepared.
[0054] S104, placing the Prussian blue positive electrode material after high temperature baking into the modified coating liquid to obtain a mixed solution, so that the oxysilane coupling agent in the modified coating liquid can be filled in the cavities of the Prussian blue positive electrode material.
[0055] It can be understood that in order to ensure that the oxysilane coupling agent can be fully and comprehensively filled in the holes of the Prussian blue positive electrode material, in one embodiment, the weight ratio of the Prussian blue positive electrode material to the oxysilane coupling agent is 100: (0.3-5), so as to ensure that the added Prussian blue positive electrode material and the oxysilane coupling agent are used in a more appropriate proportion, thereby ensuring that the added oxysilane coupling agent can be fully and comprehensively filled in the holes of the Prussian blue positive electrode material, thereby ensuring that the finally prepared modified Prussian blue positive electrode material has both good lipophilicity and hydrophobicity, and better guarantees the connection strength between the Prussian blue positive electrode material and the hydrophobic coating layer.
[0056] S105, ultrasonically operate the mixed solution. It can be understood that by ultrasonically operating the mixed solution, the oxysilane coupling agent in the modified coating liquid can be quickly and evenly dispersed on the surface of the Prussian blue positive electrode material, and as the ultrasonic operation is continuously performed, the oxysilane coupling agent in the modified coating liquid can be quickly and efficiently filled in the holes, so that the modified coating liquid can fully occupy the holes of the Prussian blue positive electrode material, which not only improves the hydrophobic property inside the Prussian blue positive electrode material, but also improves the connection strength between the hydrophobic coating layer and the Prussian blue positive electrode material.
[0057] In one embodiment, the ultrasonic operation conditions are: ultrasonic temperature 40°C to 60°C, ultrasonic frequency range 5kHz to 20kHz, to ensure that the oxysilane coupling agent in the modified coating liquid can be better filled in the cavities of the Prussian blue positive electrode material. It is worth mentioning that since there is a small amount of deionized water in the modified coating liquid, and the Prussian blue positive electrode material has a strong water absorption, the oxysilane coupling agent in the modified coating liquid can enter the cavities of the Prussian blue positive electrode material more quickly, and at the same time, with the ultrasonic operation, the oxysilane coupling agent can be filled more fully in the cavities more quickly, thereby better ensuring the connection strength between the hydrophobic coating layer and the Prussian blue positive electrode material.
[0058] S106, heating the mixed solution after ultrasonic operation in a water bath.
[0059] It can be understood that although the weight ratio of the oxysilane coupling agent to the deionized water used is controlled to be (7-45): (0.5-1), the free water in the modified coating liquid can be avoided to interfere with the filling of the oxysilane coupling agent in the modified coating liquid, but it is impossible to achieve a completely perfect effect, that is, there is still a small amount or a very small amount of free water, and these small amounts of free water will still cause the modified Prussian blue positive electrode material to collapse easily during multiple cycles. Therefore, in the present disclosure, the mixed solution after ultrasonic operation is heated in a water bath to ensure that the added oxysilane coupling agent can achieve comprehensive cross-linking with the Prussian blue positive electrode material under the conditions of a water bath, so as to form a hydrophobic coating layer with high fullness and high connection strength on the Prussian blue positive electrode material, that is, a hydrophobic coating layer is embedded on the surface of the Prussian blue positive electrode material, which better ensures the firmness of the connection between the Prussian blue positive electrode material and the hydrophobic coating layer.
[0060] It is worth mentioning that under the condition of water bath heating, the hydrolysis of the oxysilane coupling agent can be promoted. On the one hand, the free water in the modified coating liquid is consumed, effectively avoiding the presence of moisture in the hydrophobic coating layer and affecting the electrical properties of the modified Prussian blue positive electrode material; on the other hand, since the oxysilane coupling agent can increase the surface energy of the modified coating liquid during the hydrolysis process, the modified coating liquid can be more fully and comprehensively cross-linked in the pores of the Prussian blue positive electrode material, that is, a hydrophobic coating layer with high fullness and high connection strength is formed in the pores of the Prussian blue positive electrode material, so as to ensure that a modified hydrophobic Prussian blue positive electrode material with extremely low moisture content, good lipophilicity and hydrophobicity, and high connection strength is prepared.
[0061] In one embodiment, the conditions of the water bath heating operation are: a water bath is carried out in an inert atmosphere, and the temperature of the water bath is controlled at 45°C to 90°C, the water bath time is 10min to 120min, and the pH is 5 to 8, so as to ensure that the modified coating liquid can achieve more sufficient and comprehensive cross-linking at 45°C to 90°C, so as to ensure that a hydrophobic coating layer with high fullness and high connection strength is formed in the cavities of the Prussian blue positive electrode material.
[0062] S107, filtering the mixed solution after the water bath heating operation to obtain a filter residue to effectively remove the filtrate.
[0063] S108, drying the filter residue to obtain a modified hydrophobic Prussian blue positive electrode material. Specifically, the filter residue is placed in a drying oven for drying to effectively remove excess organic solvent or water, thereby ensuring that a modified hydrophobic Prussian blue positive electrode material with extremely low moisture content, good lipophilicity and hydrophobicity, and high connection strength is obtained. In addition, the filter residue is dried to ensure that the modified coating liquid can achieve more comprehensive and sufficient cross-linking, that is, it can better compensate for the small amount of incompletely cross-linked oxysilane coupling agent in the water bath heating, and further ensure the connection strength between the embedded hydrophobic coating layer and the Prussian blue positive electrode material.
[0064] In one of the embodiments, the drying conditions are a temperature of 75°C to 90°C and a time of 5h to 8h, which can not only completely remove excess organic solvent or moisture on the surface of the filter residue, but also make up for a small amount of incompletely cross-linked oxysilane coupling agent during water bath heating, so as to ensure that a modified hydrophobic Prussian blue positive electrode material with extremely low moisture content, good lipophilicity and hydrophobicity, and high connection strength is obtained.
[0065] The above-mentioned hydrophobic Prussian blue positive electrode material and its modification method first perform a high-temperature baking operation on the Prussian blue positive electrode material to effectively remove the crystal water in the Prussian blue positive electrode material and leave holes, and mix the oxysilane coupling agent, organic solvent and a small amount of deionized water to obtain a modified coating liquid to achieve the separate preparation of the modified coating liquid, effectively avoiding the problem that deionized water is directly added to the Prussian blue positive electrode material after high-temperature baking and interferes with the oxysilane coupling agent filling the holes of the Prussian blue positive electrode material. When the Prussian blue positive electrode material after high-temperature baking is placed in the modified coating liquid for ultrasonic operation, the oxysilane coupling agent in the modified coating liquid can be quickly and evenly dispersed on the surface of the Prussian blue positive electrode material, and as the ultrasonic operation is continuously performed, the oxysilane coupling agent in the modified coating liquid can be quickly and efficiently filled in the holes, so that the modified coating liquid can fully occupy the holes of the Prussian blue positive electrode material, which not only improves the hydrophobicity inside the Prussian blue positive electrode material The invention discloses a method for improving the performance of the modified coating liquid and the connection strength between the modified coating liquid and the Prussian blue positive electrode material; then the mixed liquid after the ultrasonic operation is heated in a water bath to ensure that the added oxysilane coupling agent can achieve comprehensive cross-linking with the Prussian blue positive electrode material under the condition of a water bath, so that a hydrophobic coating layer is embedded on the surface of the Prussian blue positive electrode material to form a hydrophobic coating layer, thereby ensuring that the modified Prussian blue positive electrode material has both good oleophilic and hydrophobic characteristics, so that the added modified coating liquid has the characteristics of coupling the Prussian blue positive electrode material and the positive electrode binder PVDF at the same time, so that the surface electronegative groups of the hydrophobic coating layer of the modified Prussian blue positive electrode material can produce hydrogen bonds with the fluorine atoms of the positive electrode binder PVDF, thereby improving the compatibility and dispersibility of the modified Prussian blue positive electrode material in the positive electrode slurry, thereby increasing the adhesion between the modified Prussian blue positive electrode material and the positive electrode binder PVDF, thereby improving the adhesion between the positive electrode slurry and the current collector, and thereby improving the cycle performance of the sodium ion battery.
[0066] Furthermore, since the oxysilane coupling agent of the modified coating liquid can be quickly and efficiently filled in the cavities, the baking time for preparing the modified hydrophobic Prussian blue positive electrode sheet is effectively shortened, thereby improving the production efficiency of the modified hydrophobic Prussian blue positive electrode sheet.
[0067] It is worth mentioning that the modified coating liquid is prepared separately, which effectively avoids the added deionized water from directly occupying the hole position of the Prussian blue positive electrode material, and the added deionized water is conducive to the modified coating liquid to quickly enter the hole of the Prussian blue positive electrode material. At the same time, accompanied by ultrasonic operation, the oxysilane coupling agent of the modified coating liquid can fill the hole of the Prussian blue positive electrode material more quickly, thereby ensuring that a hydrophobic coating layer with high fullness is embedded in the hole of the Prussian blue positive electrode material, thereby ensuring the connection strength between the Prussian blue positive electrode material and the hydrophobic coating layer; at the same time, with the water bath operation , which can fully consume the free water in the modified coating liquid and improve the surface energy of the modified coating liquid, so that the oxysilane coupling agent can be more fully and comprehensively cross-linked with the Prussian blue positive electrode material, thereby improving the connection strength between the modified coating liquid and the Prussian blue positive electrode material. Finally, the filter residue is dried, which not only fully removes the excess organic solvent or moisture on the surface of the filter residue, but also makes up for the small amount of oxysilane coupling agent that is not fully cross-linked during water bath heating, so as to ensure that a modified hydrophobic Prussian blue positive electrode material with extremely low moisture content, good lipophilicity and hydrophobicity, and high connection strength is obtained.
[0068] In one embodiment, the water contact angle of the modified hydrophobic Prussian blue positive electrode material is 100° to 130°, so as to ensure that the hydrophobic coating layer of the modified hydrophobic Prussian blue positive electrode material has both good lipophilicity and hydrophobicity, so that the added modified coating liquid has the characteristics of coupling the Prussian blue positive electrode material and the positive electrode binder PVDF, so that the surface electronegative groups of the hydrophobic coating layer of the modified Prussian blue positive electrode material can produce hydrogen bonds with the fluorine atoms of the positive electrode binder PVDF, thereby improving the compatibility and dispersibility of the modified Prussian blue positive electrode material in the positive electrode slurry, thereby increasing the adhesion between the modified Prussian blue positive electrode material and the positive electrode binder PVDF, thereby improving the adhesion between the positive electrode slurry and the current collector, and thereby improving the cycle performance of the sodium ion battery.
[0069] The present disclosure also provides a modified hydrophobic Prussian blue positive electrode material, which is prepared by the modification method of the hydrophobic Prussian blue positive electrode material described in any of the above embodiments. It can be understood that the modified hydrophobic Prussian blue positive electrode material prepared by the modification method of the hydrophobic Prussian blue positive electrode material disclosed in the present disclosure has an extremely low moisture content, and at the same time has good lipophilicity and hydrophobicity, thereby improving the compatibility and dispersibility of the modified Prussian blue positive electrode material in the positive electrode slurry, thereby increasing the adhesion between the modified Prussian blue positive electrode material and the positive electrode binder PVDF, thereby improving the adhesion between the positive electrode slurry and the current collector, and at the same time, the modified hydrophobic Prussian blue positive electrode material has good connection strength itself, so as to better improve the cycle performance of the sodium ion battery.
[0070] The present disclosure also provides a modified hydrophobic Prussian blue positive electrode sheet, comprising a current collector and a positive electrode slurry coated on the current collector, wherein the positive electrode slurry comprises the modified hydrophobic Prussian blue positive electrode material described in any of the above embodiments.
[0071] It can be understood that, since the modified hydrophobic Prussian blue positive electrode material prepared by the modification method of the hydrophobic Prussian blue positive electrode material disclosed in the present invention has both good lipophilicity and hydrophobicity, the compatibility and dispersibility of the modified Prussian blue positive electrode material in the positive electrode slurry are improved, thereby increasing the adhesion between the modified Prussian blue positive electrode material and the positive electrode binder PVDF, thereby improving the adhesion between the positive electrode slurry and the current collector, and at the same time, the modified hydrophobic Prussian blue positive electrode material itself has good connection strength, which better improves the cycle performance of the sodium ion battery. In addition, since the modified coating liquid fills and occupies the cavities of the Prussian blue positive electrode material, the baking time for preparing the modified hydrophobic Prussian blue positive electrode sheet is effectively shortened, thereby improving the production efficiency of the modified hydrophobic Prussian blue positive electrode sheet.
[0072] In one embodiment, the current collector may be aluminum foil.
[0073] The present disclosure also provides a sodium ion battery, comprising the modified hydrophobic Prussian blue positive electrode sheet of any of the above embodiments. It can be understood that by applying the modified hydrophobic Prussian blue positive electrode sheet prepared by the present disclosure to the sodium ion battery, the modified hydrophobic Prussian blue positive electrode material contained in the modified hydrophobic Prussian blue positive electrode sheet has good connection strength, can improve the adhesion between the positive electrode slurry and the current collector, and shorten the baking time of the modified hydrophobic Prussian blue positive electrode sheet, thereby improving the production efficiency of the sodium ion battery.
[0074] Compared with the prior art, the present invention has at least the following advantages:
[0075] 1) First, the Prussian blue positive electrode material is subjected to a high-temperature baking operation to effectively remove the crystal water in the Prussian blue positive electrode material to leave holes, and the oxysilane coupling agent, an organic solvent and a small amount of deionized water are mixed to obtain a modified coating liquid, so as to realize the separate preparation of the modified coating liquid, and effectively avoid the problem that deionized water is directly added to the Prussian blue positive electrode material after high-temperature baking and interferes with the oxysilane coupling agent filling the holes of the Prussian blue positive electrode material. When the Prussian blue positive electrode material after high-temperature baking is placed in the modified coating liquid for ultrasonic operation, the oxysilane coupling agent in the modified coating liquid can be quickly and evenly dispersed on the surface of the Prussian blue positive electrode material, and as the ultrasonic operation is continuously performed, the oxysilane coupling agent in the modified coating liquid can be quickly and efficiently filled in the holes, so that the modified coating liquid can fully occupy the holes of the Prussian blue positive electrode material, which not only improves the hydrophobicity inside the Prussian blue positive electrode material, but also improves the modified The connection strength between the coating liquid and the Prussian blue positive electrode material is improved; then the mixed liquid after the ultrasonic operation is heated in a water bath to ensure that the added oxysilane coupling agent can achieve comprehensive cross-linking with the Prussian blue positive electrode material under the condition of a water bath, so that a hydrophobic coating layer is embedded on the surface of the Prussian blue positive electrode material to form a hydrophobic coating layer, thereby ensuring that the modified Prussian blue positive electrode material has both good oleophilic and hydrophobic characteristics, so that the added modified coating liquid has the characteristics of coupling the Prussian blue positive electrode material and the positive electrode binder PVDF, so that the surface electronegative groups of the hydrophobic coating layer of the modified Prussian blue positive electrode material can produce hydrogen bonds with the fluorine atoms of the positive electrode binder PVDF, thereby improving the compatibility and dispersibility of the modified Prussian blue positive electrode material in the positive electrode slurry, thereby increasing the adhesion between the modified Prussian blue positive electrode material and the positive electrode binder PVDF, thereby improving the adhesion between the positive electrode slurry and the current collector, and thereby improving the cycle performance of the sodium ion battery.
[0076] 2) Since the oxysilane coupling agent of the modified coating liquid can be quickly and efficiently filled in the cavities, the baking time for preparing the modified hydrophobic Prussian blue positive electrode sheet is effectively shortened, thereby improving the production efficiency of the modified hydrophobic Prussian blue positive electrode sheet.
[0077] Some specific examples are given below, and if % is mentioned, it means percentage by weight. It should be noted that the following examples do not exhaust all possible situations, and the materials used in the following examples can be obtained from commercial sources unless otherwise specified.
[0078] Embodiment 1:
[0079] (1) Prussian blue positive electrode material (Prussian blue Fe4[Fe(CN)6]3, Tianjin Huasheng Chemical Reagent Co., Ltd.) was baked in an oven at 200°C for 10 h for use;
[0080] (2) γ-aminopropyltriethoxysilane (model KH-550, manufacturer: Sinopharm Chemical Reagent Co., Ltd.) was placed in anhydrous ethanol, and a small amount of deionized water was added and stirred evenly. The weight ratio of γ-aminopropyltriethoxysilane, deionized water and anhydrous ethanol was 25:1:2.5. The mixture was allowed to stand for 10 minutes to obtain a modified coating liquid.
[0081] (3) adding the Prussian blue positive electrode material (the weight ratio of the Prussian blue positive electrode material to γ-aminopropyltriethoxysilane is 100:1) baked in step (1) into the internal modified coating liquid (2) to obtain a mixed liquid;
[0082] Then the mixed solution was placed in an ultrasonic water tank and dispersed evenly (ultrasonic temperature 60°C, ultrasonic frequency range 20kHz, ultrasonic time 30min);
[0083] (4) placing the mixed solution after ultrasonic operation in a water bath and performing water bathing in an inert nitrogen atmosphere (water bath temperature 75°C, water bath time 40 min, pH 6, pH regulated by CH3COOH and NH3·H2O);
[0084] (5) filtering the mixed solution after step (4) to obtain a filter residue;
[0085] (6) placing the filter residue in a vacuum drying oven for drying (drying temperature 90° C., drying time 6 h) to obtain a modified Prussian blue positive electrode material;
[0086] (7) preparing a positive electrode slurry using the modified Prussian blue positive electrode material, positive electrode binder PVDF and conductive agent of step (6), then coating the positive electrode slurry on an aluminum foil, and then rolling and cutting the coated aluminum foil to prepare a modified Prussian blue positive electrode sheet;
[0087] (8) The modified Prussian blue positive electrode sheet is baked at high temperature to remove moisture. When the moisture content is less than 300 ppm, the baking time is recorded.
[0088] Embodiment 2:
[0089] The difference from Example 1 is that the weight ratio of the Prussian blue positive electrode material and the oxysilane coupling agent in step (3) is changed from 100:1 to 100:2, and the rest remains unchanged.
[0090] Embodiment 3:
[0091] The difference from Example 1 is that the γ-aminopropyltriethoxysilane (model KH-550) in step (2) is replaced by γ-(2,3-epoxypropyloxy)propyltrimethoxysilane (model KH-560, Sinopharm Chemical Reagent Co., Ltd.), and the rest remains unchanged.
[0092] Embodiment 4:
[0093] The difference from Example 1 is that the γ-aminopropyltriethoxysilane (model KH-550) in step (2) is replaced by γ-methacryloxypropyltrimethoxysilane (KH-570, Sinopharm Chemical Reagent Co., Ltd.), and the rest remains unchanged.
[0094] Embodiment 5:
[0095] The difference from Example 1 is that the γ-aminopropyltriethoxysilane (model KH-550) in step (2) replaces the mixture of γ-(2,3-epoxypropyloxy)propyltrimethoxysilane (KH-560) and γ-methacryloxypropyltrimethoxysilane (KH-570), and the weight ratio of γ-(2,3-epoxypropyloxy)propyltrimethoxysilane (KH-560) to γ-methacryloxypropyltrimethoxysilane (KH-570) is 1:1, and the rest remains unchanged.
[0096] Embodiment 6:
[0097] The difference from Example 1 is that the γ-aminopropyltriethoxysilane (model KH-550) in step (2) is replaced by a mixture of γ-aminopropyltriethoxysilane (KH-550) and γ-methacryloxypropyltrimethoxysilane (KH-570), and the weight ratio of γ-aminopropyltriethoxysilane (KH-550) and γ-methacryloxypropyltrimethoxysilane (KH-570) is 1:1, and the rest remains unchanged.
[0098] Embodiment 7:
[0099] The difference from Example 1 is that the γ-aminopropyltriethoxysilane (model KH-550) in step (2) is replaced by a mixture of γ-aminopropyltriethoxysilane (KH-550) and γ-(2,3-epoxypropyloxy)propyltrimethoxysilane (KH-560), and the weight ratio of γ-aminopropyltriethoxysilane (KH-550) to γ-(2,3-epoxypropyloxy)propyltrimethoxysilane (KH-560) is 1:1, and the rest remains unchanged.
[0100] Embodiment 8:
[0101] The difference from Example 1 is that the weight ratio of γ-aminopropyltriethoxysilane, deionized water and anhydrous ethanol used in step (2) is replaced from 25:1:2.5 to 7:1:0.7;
[0102] Embodiment 9:
[0103] The difference from Example 1 is that the weight ratio of γ-aminopropyltriethoxysilane, deionized water and anhydrous ethanol used in step (2) is 25:1:2.5, which is replaced by 7:0.5:0.7;
[0104] Embodiment 10:
[0105] The difference from Example 1 is that the weight ratio of γ-aminopropyltriethoxysilane, deionized water and anhydrous ethanol used in step (2) is replaced from 25:1:2.5 to 45:1:4.5.
[0106] Embodiment 11:
[0107] The difference from Example 1 is that the weight ratio of γ-aminopropyltriethoxysilane, deionized water and anhydrous ethanol used in step (2) is replaced from 25:1:2.5 to 45:0.5:4.5.
[0108] Embodiment 12:
[0109] The difference from Example 1 is that the weight ratio of the Prussian blue positive electrode material and γ-aminopropyltriethoxysilane in step (3) is changed from 100:1 to 100:0.3, and the rest remains unchanged.
[0110] Embodiment 13:
[0111] The difference from Example 1 is that the weight ratio of the Prussian blue positive electrode material and γ-aminopropyltriethoxysilane in step (3) is changed from 100:1 to 100:5, and the rest remains unchanged.
[0112] Comparative Example 1:
[0113] The difference from Example 1 is that steps (1) to (6) are omitted, and the Prussian blue positive electrode material is directly prepared into a positive electrode slurry with PVDF and a conductive agent, and then the positive electrode slurry is coated on an aluminum foil, and then the coated aluminum foil is rolled and cut to prepare a modified Prussian blue positive electrode sheet; the rest remains unchanged.
[0114] Comparative Example 2:
[0115] The difference from Example 1 is that in step (2), a small amount of deionized water is not added, and the rest remains unchanged.
[0116] Comparative Example 3:
[0117] The difference from Example 1 is that the weight ratio of γ-aminopropyltriethoxysilane, deionized water and anhydrous ethanol used in step (2) is replaced from 25:1:2.5 to 45:0.1:4.5.
[0118] Comparative Example 4:
[0119] The difference from Example 1 is that the weight ratio of the Prussian blue positive electrode material and γ-aminopropyltriethoxysilane in step (3) is changed from 100:1 to 100:0.1, and the rest remains unchanged.
[0120] Comparative Example 5:
[0121] The difference from Example 1 is that the weight ratio of the Prussian blue positive electrode material and γ-aminopropyltriethoxysilane in step (3) is changed from 100:1 to 100:6, and the rest remains unchanged.
[0122] The modified Prussian blue positive electrode sheets of Examples 1 to 13 and Comparative Examples 1 to 5 were stacked in sequence with the separator and the hard carbon negative electrode, and then the electrolyte was injected and formed to prepare a sodium ion battery. The sodium ion batteries of Examples 1 to 13 and Comparative Examples 1 to 5 were tested for peeling force, baking time, 25°C capacity retention rate and water contact angle, respectively, to obtain the experimental data in Table 1 below:
[0123] Test method:
[0124] 1. Peel force (N / m): The method for testing the peel strength between the modified Prussian blue cathode slurry and the aluminum foil includes the following specific steps:
[0125] 1) Use a knife and a ruler to prepare 3-5 test samples of the modified Prussian blue cathode sheet with a length and width of 300 mm × 25 mm;
[0126] 2) Stick a 20mm wide tape to the peel strength test board, try to keep it in the middle of the test board, and press it twice with a test roller to ensure the firmness of the tape and the test board;
[0127] 3) Tear off the paper layer on the surface of the tape, and then stick the cut test sample to the tape;
[0128] 4) Use a manual rolling roller to roll naturally in the same direction (without applying any external force) twice;
[0129] 5) After rolling, manually pre-pull the test sample to expose 1-2cm of the tape material area to ensure the stability of the peel force test;
[0130] 6) Then use a tensile testing machine to test the peeling force of the test sample, record the corresponding data and calculate the average value.
[0131] 2. Baking time / h (moisture content <300ppm), obtained by actual record statistics;
[0132] 3. 25℃ cycle test: Under 25℃ environment, leave it for 10min, charge it with 1C constant current and constant voltage to 3.70V; leave it for 10min, discharge it with 1C constant current to 2.0V;
[0133] 4. Water contact angle: Take the modified Prussian blue cathode powder of Examples 1 to 13 and Comparative Examples 1 to 5 respectively, fix them on a glass slide with double-sided tape, use a contact angle meter to test the water contact angle of the sample at five different positions, and average the contact angle data of the modified Prussian blue cathode material.
[0134] Table 1
[0135]
[0136]
[0137] Compared with Comparative Example 1, since Examples 1 to 7 are modified by the modified coating liquid, not only the baking time of the modified Prussian blue positive electrode sheet is shortened, but also the peel strength between the modified Prussian blue positive electrode slurry and the aluminum foil is improved, thereby improving the 25°C cycle retention rate of the sodium ion battery, that is, improving the cycle performance of the sodium ion battery. Among them, the comprehensive indicators of Example 6 are better.
[0138] It can be seen from Example 1 and Comparative Example 2 that since a small amount of deionized water is not added in Comparative Example 2, the fullness of the modified coating liquid filling is poor, resulting in the peel strength between the modified Prussian blue positive electrode slurry and the aluminum foil and the 25°C capacity retention rate of Comparative Example 2 being slightly worse than those of Example 1.
[0139] It can be seen from Examples 1, 8 to 11 and Comparative Example 3 that when the weight ratio of the oxysilane coupling agent of Examples 8 to 11 to deionized water is (7 to 45): (0.5 to 1), the comprehensive indicators of Examples 1 and 8 to 11 are better than those of Comparative Example 3.
[0140] It can be seen from Examples 1, 12 to 13 and Comparative Examples 4 to 5 that when the weight ratio of the Prussian blue positive electrode material and the oxysilane coupling agent used in Examples 1, 12 to 13 is 100:(0.3 to 5), the comprehensive indicators of Examples 1, 12 to 13 are better than those of Comparative Examples 4 to 5.
[0141] The above-mentioned embodiments only express several implementation methods of the present disclosure, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the disclosed patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present disclosure, and these all belong to the protection scope of the present disclosure. Therefore, the protection scope of the disclosed patent shall be subject to the attached claims.
Claims
1. A method for modifying a hydrophobic Prussian blue cathode material, characterized in that: Obtain Prussian blue cathode material; Performing a high temperature baking operation on the Prussian blue positive electrode material; The oxysilane coupling agent, the organic solvent and a small amount of deionized water are mixed to obtain a modified coating liquid; Putting the Prussian blue positive electrode material after high temperature baking into the modified coating liquid to obtain a mixed liquid; performing ultrasonic operation on the mixed solution; Heating the mixed solution after ultrasonic operation in a water bath; The mixed solution subjected to water bath heating operation is filtered to obtain filter residue; The filter residue is dried to obtain a modified hydrophobic Prussian blue positive electrode material.
2. The method for modifying the hydrophobic Prussian blue cathode material according to claim 1, characterized in that: The water contact angle of the modified hydrophobic Prussian blue positive electrode material is 100° to 130°.
3. The method for modifying the hydrophobic Prussian blue cathode material according to claim 1, characterized in that: The organic solvent is one or more of methanol, ethanol, acetone, isopropanol, n-butanol, furan, chloroform, N-methylpyrrolidone, benzene and dimethyl sulfoxide.
4. The method for modifying the hydrophobic Prussian blue cathode material according to claim 1, characterized in that: The weight ratio of the oxysilane coupling agent to deionized water is (7-45): (0.5-1).
5. The method for modifying the hydrophobic Prussian blue cathode material according to claim 1, characterized in that: The weight ratio of the Prussian blue positive electrode material to the oxysilane coupling agent is 100: (0.3-5).
6. The method for modifying the hydrophobic Prussian blue cathode material according to claim 1, characterized in that: The oxysilane coupling agent includes at least one of γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane and γ-methacryloxypropyltrimethoxysilane.
7. The method for modifying the hydrophobic Prussian blue cathode material according to claim 1, characterized in that: The conditions of the high temperature baking operation are: temperature 150°C to 230°C; time 5h to 48h; and / or, The conditions of the water bath heating operation are: conducting a water bath in an inert atmosphere, controlling the water bath temperature to 45° C. to 90° C., the water bath time to 10 min to 120 min, and the pH to 5 to 8; and / or, The weight ratio of the organic solvent to the oxysilane coupling agent is 1:(8-12).
8. A modified hydrophobic Prussian blue cathode material, characterized in that: The hydrophobic Prussian blue positive electrode material is prepared by the modification method of any one of claims 1 to 7.
9. A modified hydrophobic Prussian blue positive electrode sheet, characterized in that: It comprises a current collector and a positive electrode slurry coated on the current collector, wherein the positive electrode slurry comprises the modified hydrophobic Prussian blue positive electrode material according to claim 8.
10. A sodium ion battery, characterized in that: The invention comprises the modified hydrophobic Prussian blue positive electrode sheet as described in claim 9.
Citation Information
Patent Citations
Method for preparing super-hydrophobic modified lithium battery high nickel positive electrode material
CN108400313A
A method for modifying Prussian blue and its analogues and a sodium ion battery
CN109065883A
Surface-modified lithium ion battery positive electrode material and preparation method thereof
CN111697223A
Silane coupling agent coated modified sodium battery positive electrode material, preparation method and application
CN115939344A
Super-hydrophobic Prussian blue material as well as preparation method and application thereof
CN116040654A