Method for preparing sodium nitrate from stainless steel pickling waste liquid
Through membrane technology and chemical precipitation technology, the problems of high sludge generation and energy consumption in the treatment of stainless steel pickling waste liquid are solved, and the efficient recycling of sodium nitrate and by-product sodium chloride is achieved, and the comprehensive resource utilization of stainless steel pickling waste liquid is achieved. .
Patent Information
- Application Number
- CN202411363879.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-28
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, when dealing with stainless steel pickling waste liquid, there are problems of high sludge generation and energy consumption, and it is difficult to effectively utilize useful resources in the waste liquid.
Using membrane technology (electrodialysis + reverse osmosis) combined with chemical precipitation and regulatory crystallization technology, sodium nitrate and by-product sodium chloride are recovered through pH adjustment, multi-media filtration, electrodialysis, regulation of crystallization and reverse osmosis steps, reducing evaporation and saving energy. Reduce consumption.
The recycling and utilization of iron ions, fluorine ions and nitrate ions in stainless steel pickling waste liquid is achieved, and high-purity sodium nitrate products are obtained, which reduces energy consumption and realizes the comprehensive utilization of wastewater resources.
Smart Images

Figure CN119018912A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of comprehensive utilization of wastewater resources, in particular to a method for preparing sodium nitrate by utilizing stainless steel pickling waste liquid. Background Art
[0002] Stainless steel pickling waste liquid contains a large amount of iron ions, fluoride ions, nitrate ions, etc., and there is a lot of room for improvement in resource utilization. It is imperative to develop chemical resource recycling technology in stainless steel pickling waste liquid through technological innovation, and the recycling and utilization of these useful resources can play a positive role in water saving and emission reduction and industry upgrading. At present, stainless steel manufacturers generally use lime method to directly dispose of stainless steel pickling waste liquid by one-step neutralization and precipitation. This method will produce a large amount of sludge, the water content of the sludge is about 60%, and the content of each component in the sludge has no obvious regularity. Among them, the content of CaF2, CaO, Fe2O3, and Cr2O3 is relatively high, and the total content of valuable metals such as Cr and Fe accounts for about 10-20%. The accumulation and storage of a large amount of stainless steel sludge also causes secondary pollution. In addition, the existing technology generally recovers inorganic salt products in stainless steel pickling waste liquid by evaporation, which has the problem of high energy consumption. How to effectively treat and utilize the useful resources in stainless steel pickling waste liquid and reduce energy consumption has become a technical problem that technicians in this field need to solve urgently. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing sodium nitrate using stainless steel pickling waste liquid to solve the problems existing in the above-mentioned prior art. The present invention uses membrane technology (electrodialysis + reverse osmosis) to achieve solution concentration, reduce evaporation, save energy and reduce consumption, and at the same time combines chemical precipitation technology and controlled crystallization technology to recover the high-value sodium nitrate and byproduct sodium chloride in the waste liquid, thereby realizing the comprehensive utilization of stainless steel pickling waste liquid.
[0004] To achieve the above object, the present invention provides the following solutions:
[0005] One of the technical solutions of the present invention is a method for preparing sodium nitrate using stainless steel pickling waste liquid, comprising the following steps:
[0006] The pH of the stainless steel pickling waste liquid is adjusted to 4-6, and a precipitation reaction is performed. After the reaction is completed, the solid and liquid are separated to obtain a precipitate 1 and a filtrate 1;
[0007] The filtrate 1 is subjected to multi-media filtration to obtain a filtrate 2, and then the pH is adjusted to 7-9, and a heavy metal capture agent is added, and after the reaction is completed, the filtrate is filtered to obtain a filtrate 3;
[0008] The filler used in the multi-media filtration comprises manganese sand, activated carbon and barite.
[0009] The filtrate 3 is subjected to electrodialysis by an electrodialysis system to obtain a concentrated solution and a desalted solution; the concentrated solution is subjected to controlled crystallization to obtain sodium nitrate and a by-product of sodium chloride; the desalted solution is subjected to reverse osmosis to obtain produced water and concentrated water (reverse osmosis concentrated water).
[0010] Furthermore, the method for preparing sodium nitrate using stainless steel pickling waste liquid also includes the following steps: adding sodium hydroxide solution to the precipitate 1 to adjust the pH of the system to 12 (precipitation defluorination) to obtain a low-fluorine precipitate.
[0011] The fluorine content in the low-fluorine precipitate is less than 5 wt.%.
[0012] After the precipitation reaction, a large amount of iron ions and fluoride ions in the system are precipitated out in the form of precipitation; adjusting the pH of the precipitation 1 to 12 can further remove the fluorine in the precipitation and produce a low-fluorine precipitate.
[0013] Furthermore, the method for preparing sodium nitrate using stainless steel pickling waste liquid also includes the following steps: removing calcium and magnesium from concentrated water (reverse osmosis concentrated water), filtering to obtain filtrate 4, then adjusting the pH of filtrate 4 to neutral to obtain filtrate 5; and filtrate 5 continues to return to the electrodialysis system.
[0014] Furthermore, the calcium and magnesium are removed by lime-soda ash precipitation in batches. The specific method includes: adding calcium oxide to concentrated water to first precipitate sulfate in the system, adding sodium carbonate to the filtrate to precipitate calcium ions in the system. The relevant reaction equation is as follows:
[0015] CaO+H2O=Ca(OH)2
[0016] Ca(OH)2+Mg 2+ =Mg(OH)2↓+Ca 2+
[0017] Ca 2+ +SO4 2- =CaSO4↓
[0018] Ca 2+ +Na2CO3=Na + +CaCO3↓
[0019] Furthermore, the removal of calcium and magnesium in the concentrated water and the adjustment of the pH of the filtrate 4 to neutral are intermittent operations, which are performed every 3 to 5 hours to reduce the risk of scaling.
[0020] The step of removing calcium and magnesium from concentrated water can reduce the concentration of scaling ions to the level before enrichment, reduce the contamination of membrane components by scaling ions, and ensure the quality of related products. The filtrate can be returned to the electrodialysis system for recycling.
[0021] Furthermore, the heavy metal capture agent is an organic sulfur polymer.
[0022] Furthermore, the method further includes adding a flocculant after adding the heavy metal capture agent.
[0023] Further, the organosulfur polymer includes DTCR-1, TMT-15 or SewageARKTMT;
[0024] The flocculant includes polyaluminium chloride (PAC) and / or polyacrylamide (PAM).
[0025] Furthermore, the membrane material used in the electrodialysis includes a monovalent and divalent selective anion separation membrane; and the electrodialysis time is 4 to 6 hours.
[0026] The monovalent and divalent selective anion separation membrane can separate monovalent anions (such as Cl-, NO3-, F-) and divalent anions (such as SO4 2- ) have different permeabilities and can achieve the separation of monovalent and divalent anions.
[0027] Furthermore, the method for regulating crystallization includes evaporative crystallization and vacuum crystallization;
[0028] The temperature of the evaporation crystallization is 118-120°C; the temperature of the vacuum crystallization is 40-50°C.
[0029] Furthermore, the method for regulating crystallization specifically includes: evaporating the concentrated solution at a temperature of 118-120° C., evaporating 80 vol.% of the water, and then passing through a vacuum crystallizer to crystallize at 40-50° C. to obtain sodium nitrate, and continuing to evaporate and crystallize the filtrate at a temperature of 118-120° C. to obtain sodium chloride, and returning the mother liquor to the vacuum crystallization step.
[0030] The product quality of sodium nitrate (sodium nitrate greater than 98.0wt.%, sodium carbonate less than 0.1wt.%, sodium nitrite less than 0.1wt.%, iron less than 0.005wt.%) obtained by the method of the present invention meets the industrial sodium nitrate standard (GBT 4553-2016).
[0031] Furthermore, the stainless steel pickling waste liquid is a nitric acid-sulfuric acid-hydrofluoric acid type stainless steel pickling waste liquid.
[0032] Furthermore, the main components of the stainless steel pickling wastewater include: 10-100 g / L NO3 - , 10~20g / L F-, 1~10g / L SO4 2- , 50~500mg / L Cl-, 5~40g / L Fe 3+ 、Cr below 3g / L 3+ .
[0033] The iron and fluorine in the stainless steel pickling waste liquid of the present invention can be separated in the form of precipitation by adjusting the pH; the nitrate ion can be concentrated by electrodialysis and then recovered by adjusting the crystallization to obtain the sodium nitrate product; the produced water and evaporated condensed water obtained by further processing by reverse osmosis technology can be collected and reused.
[0034] The present invention discloses the following technical effects:
[0035] (1) The method for preparing sodium nitrate using stainless steel pickling waste liquid of the present invention can extract and recycle iron ions, fluoride ions, nitrate ions and the like in the stainless steel pickling waste liquid in the form of inorganic substances to obtain a sodium nitrate product with high value.
[0036] (2) The present invention separates ferrofluoride by chemical precipitation; separates monovalent and divalent anions in the system by electrodialysis; prepares sodium nitrate and byproduct sodium chloride by regulating crystallization; produces water by reverse osmosis, and the concentrated water obtained by reverse osmosis is returned to the electrodialysis system for recycling after calcium and magnesium are removed, thereby realizing the comprehensive utilization of stainless steel pickling wastewater resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0038] Figure 1 The present invention is a schematic flow chart of a method for preparing sodium nitrate by utilizing stainless steel pickling waste liquid. DETAILED DESCRIPTION
[0039] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0040] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0041] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0042] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0043] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0044] The composition and content of the stainless steel pickling waste liquid (nitric acid-sulfuric acid-hydrofluoric acid type stainless steel pickling waste liquid) treated by the present invention are shown in Table 1.
[0045] Table 1 Composition and content of stainless steel pickling waste liquid
[0046]
[0047]
[0048] Example 1
[0049] A method for preparing sodium nitrate using stainless steel pickling waste liquid:
[0050] (1) Precipitation reaction
[0051] Solid NaOH was added to the stainless steel pickling waste liquid to adjust the pH value to 5, and a precipitation reaction was carried out under stirring (time was 2 hours). After the reaction was completed, the solid-liquid separation was carried out to obtain filtrate 1 and precipitate 1. Sodium hydroxide solution (concentration was 2 mol / L) was added to the precipitate 1, and the pH value was adjusted to 12 (precipitation defluorination) to obtain a low-fluorine precipitate. The main components of the low-fluorine precipitate were iron and fluorine, with iron accounting for 39.8% of the mass of the low-fluorine precipitate and fluorine accounting for 4.1% of the mass of the low-fluorine precipitate.
[0052] (2) Multi-media filtration
[0053] The filtrate 1 was adjusted to neutrality and then filtered through a multi-media filter (manganese sand + activated carbon + barite) to obtain a filtrate 2.
[0054] Among them, the particle size of manganese sand is 2-4 mm; the particle size of activated carbon is 0.5-2 mm; the particle size of barite is 4-8 mm; the mass ratio of manganese sand, activated carbon and barite is 5:3:2.
[0055] The key elements in filtrate 2 were detected and the results are shown in Table 2.
[0056] Table 2 Key elements in filtrate 2
[0057] Element Fe ions Cr ions F ions Ion concentration (mg / L) 2.2 1.32 34.8
[0058] It can be seen from Table 2 that after filtering through the multi-media filter, a small amount of iron ions, chromium ions and fluoride ions remain in the solution.
[0059] (3) pH adjustment
[0060] Sodium hydroxide was added to filtrate 2 to adjust the pH to 8, and then a heavy metal capture agent DTCR-1 (the dosage of DTCR-1 was 2 mg / L) was added to further remove heavy metal ions. After the reaction was completed, the mixture was filtered to obtain filtrate 3.
[0061] The key elements in filtrate 3 were detected and the results are shown in Table 3.
[0062] Table 3 Key elements in filtrate 3
[0063] Element Fe ions Cr ions F ions Ion concentration (mg / L) - - 24.2
[0064] As can be seen from Table 3, after pH adjustment and heavy metal capture, iron ions and chromium ions were not detected in the solution, and the fluoride ion content was further reduced.
[0065] (4) Electrodialysis
[0066] The filtrate 3 was subjected to electrodialysis, and the membrane material used in the electrodialysis was a monovalent and divalent selective anion separation membrane, to obtain a concentrated solution and a desalted solution; wherein, the initial current of the electrodialysis was 3A, the initial voltage was 11V, and the reaction time was 4h.
[0067] The components of the desalted liquid and the concentrated liquid were analyzed and the results are shown in Table 4.
[0068] Table 4 Composition of desalted liquid and concentrated liquid
[0069]
[0070] (5) Crystallization Control
[0071] The concentrated solution obtained by electrodialysis is evaporated at a temperature of 120°C (primary evaporation). When the amount of evaporated water is 80 vol.%, the heating is stopped and the solution is transferred to a vacuum crystallization device. The temperature is controlled at 40°C and the solid-liquid separation (centrifugal separation) is performed to obtain sodium nitrate. The purity of the sodium nitrate product is 98.3% (less than 0.01% sodium carbonate, less than 0.01% ammonium nitrite, and no iron is detected). The product quality meets the industrial sodium nitrate standard (GBT4553-2016).
[0072] The obtained filtrate is evaporated further (secondary evaporation) at an evaporation temperature of 120°C. After heat preservation and sedimentation, it is centrifuged while hot to separate the precipitated crystals into sodium chloride. The mother liquor is returned to the vacuum crystallization step.
[0073] (6) Reverse Osmosis
[0074] The desalted liquid obtained by electrodialysis was subjected to reverse osmosis treatment to obtain concentrated water and produced water, with a production water recovery rate of 60 vol.%.
[0075] The components of concentrated water and produced water were analyzed and the results are shown in Table 5.
[0076] Table 5 Composition of concentrated water and produced water
[0077]
[0078] (7) Calcium and magnesium removal and neutralization reaction
[0079] First, calcium oxide is added to the concentrated water obtained by reverse osmosis to precipitate sulfate, and then sodium carbonate is added to precipitate calcium ions to remove the scaling ions to the concentration level before enrichment. Filtrate 4 is obtained by filtration, and the pH of filtrate 4 is adjusted to neutral with hydrochloric acid to obtain filter residue and filtrate 5. Filtrate 5 is returned to the electrodialysis system for recycling. This step is an intermittent operation, and calcium and magnesium are removed every 4 hours. The flow diagram of the method for comprehensive utilization of stainless steel pickling wastewater is shown in Figure 1 .
[0080] Example 2
[0081] A method for preparing sodium nitrate using stainless steel pickling waste liquid:
[0082] (1) Precipitation reaction
[0083] Solid NaOH was added to the stainless steel pickling waste liquid to adjust the pH value to 5, and a precipitation reaction was carried out under stirring (for 2 hours). After the reaction was completed, the solid-liquid was separated to obtain filtrate 1 and precipitate 1. Sodium hydroxide solution (concentration of 2 mol / L) was added to precipitate 1, and the pH value was adjusted to 11.8 (precipitation defluorination) to obtain a low-fluorine precipitate. The main components of the low-fluorine precipitate were iron and fluorine, and fluorine accounted for 4.5% of the mass of the low-fluorine precipitate.
[0084] (2) Multi-media filtration
[0085] The filtrate 1 was adjusted to neutrality and then filtered through a multi-media filter (manganese sand + activated carbon + barite) to obtain a filtrate 2.
[0086] Among them, the particle size of manganese sand is 2-4 mm; the particle size of activated carbon is 0.5-2 mm; the particle size of barite is 4-8 mm; the mass ratio of manganese sand, activated carbon and barite is 5:3:2.
[0087] (3) pH adjustment
[0088] Sodium hydroxide was added to filtrate 2 to adjust the pH to 8, and then a heavy metal capture agent TMT-15 (the dosage of TMT-15 was 2 mg / L) was added to further remove heavy metal ions. After the reaction was completed, the solution was filtered to obtain filtrate 3.
[0089] (4) Electrodialysis
[0090] The filtrate 3 was subjected to electrodialysis, and the membrane material used in the electrodialysis was a monovalent and divalent selective anion separation membrane to separate monovalent and divalent ions to obtain a concentrated solution and a desalted solution; wherein the initial current of the electrodialysis was 3A, the initial voltage was 11V, and the reaction time was 5h.
[0091] (5) Crystallization Control
[0092] The concentrated solution obtained by electrodialysis is evaporated at a temperature of 120°C (primary evaporation). When the amount of evaporated water is 80 vol.%, the heating is stopped and the solution is transferred to a vacuum crystallization device. The temperature is controlled at 40°C and the solid-liquid separation is performed to obtain sodium nitrate. The purity of the sodium nitrate product is 98.6% (sodium carbonate is less than 0.01%, ammonium nitrite is less than 0.01%, and iron is not detected). The product quality meets the industrial sodium nitrate standard (GBT4553-2016).
[0093] The obtained filtrate is evaporated further (secondary evaporation) at an evaporation temperature of 120°C. After heat preservation and sedimentation, it is filtered and separated while hot. The precipitated crystals are sodium chloride. The mother liquor is returned to the vacuum crystallization step.
[0094] (6) Reverse Osmosis
[0095] The desalted liquid obtained by electrodialysis is subjected to reverse osmosis treatment to obtain concentrated water and produced water.
[0096] (7) Calcium and magnesium removal and neutralization reaction
[0097] First, calcium oxide is added to the concentrated water obtained by reverse osmosis to precipitate sulfate, and then sodium carbonate is added to precipitate calcium ions to remove the scaling ions to the concentration level before enrichment, and filtrate 4 is obtained by filtration. The pH of filtrate 4 is adjusted to neutral with hydrochloric acid to obtain filter residue and filtrate 5, and filtrate 5 is returned to the electrodialysis system for recycling. This step is an intermittent operation, and calcium and magnesium removal is performed every 3 hours.
[0098] Example 3
[0099] A method for preparing sodium nitrate using stainless steel pickling waste liquid:
[0100] (1) Precipitation reaction
[0101] Solid NaOH was added to the stainless steel pickling waste liquid to adjust the pH value to 5, and a precipitation reaction was carried out under stirring (for 2 hours). After the reaction was completed, the solid-liquid was separated to obtain filtrate 1 and precipitate 1. Sodium hydroxide solution (concentration of 2 mol / L) was added to precipitate 1, and the pH value was adjusted to 11.5 (precipitation defluorination) to obtain a low-fluorine precipitate. The main components of the low-fluorine precipitate were iron and fluorine, and fluorine accounted for 4.8% of the mass of the low-fluorine precipitate.
[0102] (2) Multi-media filtration
[0103] The filtrate 1 was adjusted to neutrality and then filtered through a multi-media filter (manganese sand + activated carbon + barite) to obtain a filtrate 2.
[0104] Among them, the particle size of manganese sand is 2-4 mm; the particle size of activated carbon is 0.5-2 mm; the particle size of barite is 4-8 mm; the mass ratio of manganese sand, activated carbon and barite is 5:3:2.
[0105] (3) pH adjustment
[0106] Sodium hydroxide was added to filtrate 2 to adjust the pH to 8, and then heavy metal capture agent TMT-15 (the dosage of TMT-15 was 2 mg / L) and flocculant polyaluminium chloride (PAC) (the dosage of polyaluminium chloride (PAC) was 10 mg / L) were added to further remove heavy metal ions. After the reaction was completed, the mixture was filtered to obtain filtrate 3.
[0107] (4) Electrodialysis
[0108] The filtrate 3 was subjected to electrodialysis, and the membrane material used in the electrodialysis was a monovalent and divalent selective anion separation membrane to separate monovalent and divalent ions to obtain a concentrated solution and a desalted solution; wherein the initial current of the electrodialysis was 3A, the initial voltage was 11V, and the reaction time was 6h.
[0109] (5) Crystallization Control
[0110] The concentrated solution obtained by electrodialysis is evaporated at a temperature of 120°C (primary evaporation). When the amount of evaporated water is 80 vol.%, the heating is stopped and the solution is transferred to a vacuum crystallization device. The temperature is controlled at 40°C and the solid-liquid separation is performed to obtain sodium nitrate. The purity of the sodium nitrate product is 98.8% (sodium carbonate is less than 0.01%, ammonium nitrite is less than 0.01%, and iron is not detected). The product quality meets the industrial sodium nitrate standard (GBT4553-2016).
[0111] The obtained filtrate is evaporated further (secondary evaporation) at an evaporation temperature of 120°C. After heat preservation and sedimentation, it is filtered and separated while hot. The precipitated crystals are sodium chloride. The mother liquor is returned to the vacuum crystallization step.
[0112] (6) Reverse Osmosis
[0113] The desalted liquid obtained by electrodialysis is subjected to reverse osmosis treatment to obtain concentrated water and produced water.
[0114] (7) Calcium and magnesium removal and neutralization reaction
[0115] First, calcium oxide is added to the concentrated water obtained by reverse osmosis to precipitate sulfate, and then sodium carbonate is added to precipitate calcium ions to remove the scaling ions to the concentration level before enrichment, and filtrate 4 is obtained by filtration. The pH is adjusted to neutral to obtain filter residue and filtrate 5, and filtrate 5 is returned to the electrodialysis system for recycling. This step is an intermittent operation, and calcium and magnesium removal is performed every 3.5 hours.
[0116] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing sodium nitrate using stainless steel pickling waste liquid, characterized in that: The following steps are involved: The pH of the stainless steel pickling waste liquid is adjusted to 4-6, and a precipitation reaction is performed. After the reaction is completed, the solid and liquid are separated to obtain a precipitate 1 and a filtrate 1; The filtrate 1 is subjected to multi-media filtration to obtain a filtrate 2, and then the pH is adjusted to 7-9, and a heavy metal capture agent is added, and after the reaction is completed, the filtrate is filtered to obtain a filtrate 3; The filtrate 3 is subjected to electrodialysis to obtain a concentrated solution and a desalted solution; the concentrated solution is subjected to controlled crystallization to obtain sodium nitrate and a by-product of sodium chloride; the desalted solution is subjected to reverse osmosis to obtain produced water and concentrated water.
2. The method according to claim 1, characterized in that The following steps are also included: Sodium hydroxide solution was added to the precipitate 1 to adjust the pH of the system to 12 to obtain a low-fluorine precipitate.
3. The method according to claim 1, characterized in that The following steps are also included: Calcium and magnesium are removed from the concentrated water, and filtrate 4 is obtained after filtration. Then, the pH of filtrate 4 is adjusted to neutral to obtain filtrate 5; filtrate 5 is returned to the electrodialysis system.
4. The method according to claim 1, characterized in that The heavy metal capture agent is an organic sulfur polymer.
5. The method according to claim 4, characterized in that It also includes adding a flocculant after adding a heavy metal capture agent.
6. The method according to claim 5, characterized in that The organosulfur polymer includes DTCR-1, TMT-15 or SewageARKTMT; The flocculant includes polyaluminium chloride and / or polyacrylamide.
7. The method according to claim 1, characterized in that The membrane material used in the electrodialysis includes a divalent selective anion separation membrane.
8. The method according to claim 1, characterized in that The method for regulating crystallization includes evaporative crystallization and vacuum crystallization; The temperature of the evaporation crystallization is 118-120°C; the temperature of the vacuum crystallization is 40-50°C.
9. The method according to claim 1, characterized in that: The stainless steel pickling waste liquid is a nitric acid-sulfuric acid-hydrofluoric acid type stainless steel pickling waste liquid.