Recycling method of waste lithium iron phosphate positive electrode material

By recycling Fe, P and Li elements in the waste lithium iron phosphate positive electrode material in steps, forming Na4Fe3(PO4)2P2O7 positive electrode material, solving the environmental pollution and resource waste problems in the recycling of waste lithium-ion batteries, and achieving efficient and green Recycled and reused, the resulting material has high specific capacity and excellent circulation properties.

CN119018938APending Publication Date: 2024-11-26WUHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410909174.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively recycle and reuse precious metals and toxic electrolyte salts in waste lithium-ion batteries, resulting in environmental pollution and waste of resources.

Method used

By recycling the used lithium iron phosphate positive electrode material in steps, Fe and P elements are recovered using leaching agent and precipitant, Li elements are recovered in combination with sodium ion exchange resin, and Na4Fe3(PO4)2P2O7 positive electrode material is formed, achieving green closed-loop recycling and High value conversion of low value added products.

Benefits of technology

The high leaching rate and full recycling of Li, Fe and P elements have been achieved. The Na4Fe3(PO4)2P2O7 positive electrode material produced has high specific capacity, stable cycle and superior rate performance. It is simple and easy to scale and is suitable for industrialization. Recycle and regenerate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018938A_ABST
    Figure CN119018938A_ABST
Patent Text Reader

Abstract

The invention provides a recycling and reusing method of a waste lithium iron phosphate positive electrode material, which comprises the following steps: adding a leaching agent into positive electrode powder obtained by treating the waste lithium iron phosphate positive electrode material, leaching and recycling Fe element after wet ball milling to obtain precipitated iron oxide, adding a precipitator into filtrate to recycle part of P element to obtain iron phosphate, according to the method, the Li element is recovered from the residual solution through sodium type ion exchange resin, and finally, the Na4Fe3 (PO4) 2P2O7 positive electrode material is synthesized by utilizing the recovered solution and recovered products of the Fe element and the P element, so that the green closed-loop recovery of the waste LiFePO4 battery positive electrode material and the high-value conversion of low-added-value products are realized. The recycling process is simple and easy to implement, high in element recycling rate, good in economic benefit and environmentally friendly, and large-scale recycling of the waste lithium iron phosphate battery positive electrode material is expected to be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of recycling and regenerating waste lithium-ion battery positive electrode materials, and in particular to a method for recycling and reusing waste lithium iron phosphate positive electrode materials. Background Art

[0002] Energy is the material basis for the survival and development of human society, and the replacement of energy structure is the main driving force for the progress of human civilization. As the core of the new energy industry, lithium-ion batteries have an indispensable position in transportation, energy storage, consumption, and special fields due to their high energy density, high discharge voltage, excellent cycle performance, no memory effect, and good safety.

[0003] In recent years, the price of lithium raw materials has been rising, and the market demand has continued to expand. Since the expiration time of lithium-ion battery products is generally 3-10 years, a large number of lithium-ion batteries have been retired. Retired lithium-ion batteries not only contain a variety of heavy metals such as cobalt, nickel, and manganese, but also contain toxic electrolyte salts such as LiPF6, LiBF4 or LiClO4. If they are not properly handled, they will inevitably cause environmental pollution and waste of resources. Therefore, researching and developing high-economic-efficiency, green and environmentally friendly lithium-ion battery recycling processes to achieve the "internal circulation" of lithium resources can not only avoid environmental pollution and generate higher economic benefits, but also maintain energy security and provide support for the stable supply and safety of mineral resources. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a method for recycling and reusing waste lithium iron phosphate positive electrode materials, respectively recovering the Fe element, P element and the more expensive lithium element in the waste lithium iron phosphate positive electrode materials, and similarly utilizing the recycling liquid and the recycling products of the Fe element and the P element to synthesize the Na4Fe3(PO4)2P2O7 positive electrode material, thereby realizing the green closed-loop recycling of waste LiFePO4 battery positive electrode materials and the high-value conversion of low value-added products.

[0005] The present invention provides the following technical solutions:

[0006] The present invention provides a method for recycling waste lithium iron phosphate positive electrode materials, comprising the following steps:

[0007] S1. Processing the waste lithium iron phosphate battery positive electrode sheet to obtain waste positive electrode powder;

[0008] S2, adding a leaching agent to the waste positive electrode powder, wet ball milling and leaching to recover the Fe element to obtain precipitated iron oxide, and adding a precipitating agent to the filtrate to recover part of the P element to obtain iron phosphate;

[0009] S3, the remaining solution of step S2 is used to recover the Li element through a sodium type ion exchange resin;

[0010] S4, measuring the Na and P element contents of the residual solution after the replacement recovery in step S3 by ICP, adding a carbon source, and recovering the obtained iron oxide and / or iron phosphate, so that the final molar ratio of Na:Fe:P in the suspension is 4:3:4, and spray drying to obtain a Na4Fe3(PO4)2P2O7 precursor;

[0011] S5. The precursor is calcined under the protection of an inert atmosphere to obtain Na4Fe3(PO4)2P2O7 positive electrode material.

[0012] The present invention recovers the elements in the waste lithium iron phosphate positive electrode material in steps with a high recovery rate. The remaining recovery liquid after recovery can be added with recovered iron and phosphorus recovery products, supplemented with some carbon sources, and then synthesized into Na4Fe3(PO4)2P2O7 positive electrode material, thereby realizing the green closed-loop recovery of waste LiFePO4 battery positive electrode materials and the high-value conversion of low value-added products.

[0013] Furthermore, step S1 includes heat-treating the waste lithium iron phosphate battery positive electrode sheet, stripping it from the current collector to obtain the waste positive electrode material, and further calcining and crushing the waste positive electrode material to obtain the waste positive electrode powder. Specifically, the waste lithium iron phosphate battery positive electrode sheet is calcined at 400° C. for 1 hour, then stripped from the positive electrode collector, and then calcined at 600-700° C. for 3-5 hours to obtain the waste positive electrode powder.

[0014] Furthermore, in step S2, the leaching solution is oxalic acid, and the molar ratio of the waste positive electrode powder to oxalic acid is 1:1.

[0015] Furthermore, the leaching time after wet ball milling is 1 to 4 hours.

[0016] Furthermore, the precipitant is aqueous ammonia.

[0017] Furthermore, the step S3 also includes adding sodium carbonate solution to the replaced ion exchange resin for regeneration to obtain lithium carbonate.

[0018] Furthermore, the carbon source is one of citric acid and oxalic acid or a mixture of two or more thereof.

[0019] Furthermore, in step S4, another phosphorus source is added, and the phosphorus source is diammonium phosphate.

[0020] Furthermore, in step S4, the spray drying feed rate is 6%, the air intake is 80%, and the spray pyrolysis temperature is 110°C.

[0021] Furthermore, in step S5, the inert atmosphere is argon, hydrogen or a mixture of the two.

[0022] The present invention has the following beneficial effects:

[0023] 1. The recovery method of the present invention realizes high leaching rate and full recycling of Li, Fe and P elements, and utilizes the recovery liquid and the recovery products of Fe and P elements to synthesize Na4Fe3(PO4)2P2O7 positive electrode material, thus realizing high-value conversion of low value-added recovery products;

[0024] 2. The Na4Fe3(PO4)2P2O7 cathode material obtained by the present invention has high specific capacity, stable cycle and excellent rate performance;

[0025] 3. The recycling and reuse process of waste lithium iron phosphate positive electrode materials of the present invention is simple and easy to scale up, and is suitable for industrial recycling and regeneration of waste lithium iron phosphate battery positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 The XRD diagram of the iron oxide recovered from Examples 1 to 4 of the present invention;

[0028] Figure 2 This is a SEM image of the iron phosphate recovered from Example 2 of the present invention;

[0029] Figure 3 This is a lithium extraction curve diagram of resins in Examples 1 to 3 of the present invention;

[0030] Figure 4 This is a regeneration curve diagram of the resin after replacement in Example 3 of the present invention;

[0031] Figure 5 The XRD spectrum of the Na4Fe3(PO4)2P2O7(NFPP) material prepared in Example 4 of the present invention;

[0032] Figure 6 This is a charge and discharge curve diagram of the Na4Fe3(PO4)2P2O7 material prepared in Example 4 of the present invention as a positive electrode material. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The embodiment of the present invention provides a method for recycling waste lithium iron phosphate positive electrode materials, comprising the following steps:

[0035] S1. Processing the waste lithium iron phosphate battery positive electrode sheet to obtain waste positive electrode powder;

[0036] S2, adding a leaching agent to the waste positive electrode powder, wet ball milling and leaching to recover the Fe element to obtain precipitated iron oxide, and adding a precipitating agent to the filtrate to recover part of the P element to obtain iron phosphate;

[0037] S3, the remaining solution of step S2 is used to recover the Li element through a sodium type ion exchange resin;

[0038] S4, measuring the Na and P element contents of the residual solution after the replacement recovery in step S3 by ICP, adding a carbon source, and recovering the obtained iron oxide and / or iron phosphate, so that the final molar ratio of Na:Fe:P in the suspension is 4:3:4, and spray drying to obtain a Na4Fe3(PO4)2P2O7 precursor;

[0039] S5. The precursor is calcined under the protection of an inert atmosphere to obtain Na4Fe3(PO4)2P2O7 positive electrode material.

[0040] Firstly, the waste lithium iron phosphate battery positive electrode sheet is heat-treated, and the waste positive electrode material is obtained by stripping it from the current collector, and then the waste positive electrode material is calcined and crushed to obtain the waste positive electrode powder;

[0041] The waste cathode powder is mixed with dihydrated oxalic acid and wet ball milled to obtain a uniform mixture, which is then leached and separated to obtain an iron oxide precipitate. After removing the precipitate, ammonia water as a precipitant is added to the filtrate to obtain an iron phosphate precipitate and a colorless transparent liquid. The specific reaction equation is as follows:

[0042] 12LiFePO4+3O2=4Li3Fe2(PO4)3+2Fe2O3 (1)

[0043] Li3Fe 2( PO4)3+3H2C2O4=Li2[Fe(C2O4)2]+Fe(H2PO4)2+LiH2PO4+2CO2 (2)

[0044] 2Li2[Fe(C2O4)2]+2Fe(H2PO4)2+2LiH2PO4+O2+5NH3·H2O=

[0045] 4FePO4+3Li2C2O4+(NH4)2C2O4+NH4H2PO4+(NH4)2HPO4+7H2O(3)

[0046] Then, ion exchange resin is added to the colorless transparent liquid to replace the Li element in the solution for multiple times; the replaced resin is regenerated by adding sodium carbonate solution to obtain Li2CO3, and the regenerated resin is recycled;

[0047] To the remaining liquid after replacement recovery, add additional carbon source and recovered iron oxide and / or iron phosphate to make the final molar ratio of the sodium source, iron source and phosphorus source in the suspension be 4:3:4, spray dry to obtain Na4Fe3(PO4)2P2O7 precursor, and finally calcine the precursor under inert atmosphere to obtain Na4Fe3(PO4)2P2O7 positive electrode material.

[0048] When only iron oxide is added as an iron source, another phosphorus source is added as a supplement, and the phosphorus source is ammonium dihydrogen phosphate.

[0049] Example 1

[0050] The specific process of the method for recycling and reusing waste lithium iron phosphate positive electrode materials in this embodiment is as follows:

[0051] (1) calcining the waste lithium iron phosphate battery positive electrode sheet at 400° C. for 1 h in an air atmosphere, peeling it from the positive electrode current collector to obtain the waste positive electrode material, calcining the waste positive electrode material at 600° C. for 3 h in an air atmosphere, and then crushing it in a mortar to obtain the waste positive electrode powder;

[0052] (2) Weighing equimolar amounts of waste cathode powder (1 g) and dihydrated oxalic acid (0.8 g) and mixing them, adding 1 g of deionized water as a ball milling medium, and wet milling them in a planetary ball mill for 2 h to obtain a uniform mixture;

[0053] (3) adding deionized water to the mixture and leaching for 1 hour, and centrifuging to obtain a red iron oxide precipitate;

[0054] (4) Add 1.6 mL of aqueous ammonia to the remaining green clear liquid, stir thoroughly, and filter to obtain iron phosphate precipitate and a colorless transparent solution;

[0055] (5) Add 1 g of sodium resin to the colorless transparent solution and repeatedly replace the Li + After the replacement is completed, the resin is regenerated with sodium carbonate solution, and the precipitate in the flushing liquid is separated to obtain Li2CO3. The regenerated resin can be recycled;

[0056] (6) The element content (Na:P=3:1) in the remaining solution was measured by ICP, and the recovered iron phosphate precipitate was added to make the molar ratio of the elements Na:Fe:P in the mixed solution 4:3:4. At the same time, an equal molar amount of monohydrated citric acid was added according to the theoretical output of Na4Fe3(PO4)2P2O7, and the mixed slurry was sand-milled in a sand mill for 5 h, and a Na4Fe3(PO4)2P2O7 precursor was obtained using a spray dryer;

[0057] (7) The precursor is placed in a tubular furnace and calcined at 550°C for 10 h under the protection of high-purity argon to obtain Na4Fe3(PO4)2P2O7 positive electrode material.

[0058] Example 2

[0059] The specific process of the method for recycling and reusing waste lithium iron phosphate positive electrode materials in this embodiment is as follows:

[0060] (1) calcining the waste lithium iron phosphate battery positive electrode sheet at 400° C. for 1 h in an air atmosphere, peeling it from the positive electrode current collector to obtain the waste positive electrode material, calcining the waste positive electrode material at 600° C. for 4 h in an air atmosphere, and then crushing it in a mortar to obtain the waste positive electrode powder;

[0061] (2) Weighing equimolar amounts of waste cathode powder (2 g) and dihydrated oxalic acid (1.6 g) and mixing them, adding 2 g of deionized water as a ball milling medium, and wet milling them in a planetary ball mill for 2 h to obtain a uniform mixture;

[0062] (3) adding deionized water to the mixture and leaching for 2 h, and centrifuging to obtain a red iron oxide precipitate;

[0063] (4) Add 3.2 mL of aqueous ammonia to the remaining green clear liquid, stir thoroughly, and filter to obtain iron phosphate precipitate and a colorless transparent solution;

[0064] (5) Add 2 g of sodium resin to the colorless transparent solution and repeatedly replace the Li + After the replacement is completed, the resin is regenerated with sodium carbonate solution, and the precipitate in the flushing liquid is separated to obtain Li2CO3. The regenerated resin can be recycled;

[0065] (6) The element content (Na:P=3:1) in the remaining solution was measured by ICP, and the recovered iron oxide precipitate was added, and ammonium dihydrogen phosphate was added as a phosphorus source to make the molar ratio of the elements Na:Fe:P in the mixed solution 4:3:4. At the same time, an equal molar amount of monohydrated citric acid was added according to the theoretical output of Na4Fe3(PO4)2P2O7, and the mixed slurry was sand-milled in a sand mill for 5 hours, and a Na4Fe3(PO4)2P2O7 precursor was obtained using a spray dryer;

[0066] (7) The precursor is placed in a tubular furnace and calcined at 550°C for 10 h under the protection of high-purity argon to obtain Na4Fe3(PO4)2P2O7 positive electrode material.

[0067] Example 3

[0068] The specific process of the method for recycling and reusing waste lithium iron phosphate positive electrode materials in this embodiment is as follows:

[0069] (1) calcining the waste lithium iron phosphate battery positive electrode sheet at 400° C. for 1 h in an air atmosphere, peeling it from the positive electrode current collector to obtain the waste positive electrode material, calcining the waste positive electrode material at 700° C. for 5 h in an air atmosphere, and then crushing it in a mortar to obtain the waste positive electrode powder;

[0070] (2) Weighing equimolar amounts of waste cathode powder (3 g) and dihydrated oxalic acid (2.4 g) and mixing them, adding 3 g of deionized water as a ball milling medium, and wet milling them in a planetary ball mill for 2 h to obtain a uniform mixture;

[0071] (3) adding deionized water to the mixture and leaching for 3 h, and centrifuging to obtain a red iron oxide precipitate;

[0072] (4) Add 4.8 mL of aqueous ammonia to the remaining green clear liquid, stir thoroughly, and filter to obtain iron phosphate precipitate and a colorless transparent solution;

[0073] (5) Add 4 g of sodium resin to the colorless transparent solution and repeatedly replace the Li + After the replacement is completed, the resin is regenerated with sodium carbonate solution, and the precipitate in the flushing liquid is separated to obtain Li2CO3. The regenerated resin can be recycled;

[0074] (6) The element content (Na:P=3:1) in the remaining solution was measured by ICP, and the recovered iron oxide and iron phosphate precipitate were added to make the molar ratio of the elements Na:Fe:P in the mixed solution 4:3:4. At the same time, an equal molar amount of monohydrated citric acid was added according to the theoretical output of Na4Fe3(PO4)2P2O7, and the mixed slurry was sand-milled in a sand mill for 5 h, and a Na4Fe3(PO4)2P2O7 precursor was obtained using a spray dryer;

[0075] (7) The precursor is placed in a tubular furnace and calcined at 550°C for 10 h under the protection of high-purity argon to obtain Na4Fe3(PO4)2P2O7 positive electrode material.

[0076] Example 4

[0077] The specific process of the method for recycling and reusing waste lithium iron phosphate positive electrode materials in this embodiment is as follows:

[0078] (1) calcining the waste lithium iron phosphate battery positive electrode sheet at 400° C. for 1 h in an air atmosphere, peeling it from the positive electrode current collector to obtain the waste positive electrode material, calcining the waste positive electrode material at 700° C. for 5 h in an air atmosphere, and then crushing it in a mortar to obtain the waste positive electrode powder;

[0079] (2) Weighing equimolar amounts of waste cathode powder (5 g) and dihydrated oxalic acid (4 g) and mixing them, adding 1 g of deionized water as a ball milling medium, and wet milling them in a planetary ball mill for 2 h to obtain a uniform mixture;

[0080] (3) adding deionized water to the mixture and leaching for 1 hour, and centrifuging to obtain a red iron oxide precipitate;

[0081] (4) Add 8 mL of aqueous ammonia to the remaining green clear liquid, stir thoroughly, and filter to obtain iron phosphate precipitate and a colorless transparent solution;

[0082] (5) Add 2 g of sodium resin to the colorless transparent solution and repeatedly replace the Li + After the replacement is completed, the resin is regenerated with sodium carbonate solution, and the precipitate in the flushing liquid is separated to obtain Li2CO3. The regenerated resin can be recycled;

[0083] (6) The element content (Na:P=3:1) in the remaining solution was measured by ICP, and the recovered iron phosphate precipitate was added to make the molar ratio of the elements Na:Fe:P in the mixed solution 4:3:4. At the same time, an equal molar amount of monohydrated citric acid was added according to the theoretical output of Na4Fe3(PO4)2P2O7, and the mixed slurry was sand-milled in a sand mill for 5 h, and a Na4Fe3(PO4)2P2O7 precursor was obtained using a spray dryer;

[0084] (7) The precursor is placed in a tubular furnace and calcined at 550°C for 10 h under the protection of high-purity argon to obtain Na4Fe3(PO4)2P2O7 positive electrode material.

[0085] The iron oxide recovered in Examples 1 to 4 was subjected to XRD analysis, and the results are shown in Figure 1 , it can be seen that the recovered product is completely consistent with the standard spectrum, proving the complete crystal structure and high purity of the product.

[0086] See also Figure 2 , is the SEM of the iron phosphate recovered in Example 2. It can be seen that the recovered product has a uniform morphology and fine particle size.

[0087] See also Figure 3 , is the equilibrium curve of lithium extraction by ion exchange resin in Examples 1 to 3. It can be seen that the ion exchange resin can efficiently replace the lithium ions in the solution and fully recover the Li element. Figure 4 , is the regeneration equilibrium curve diagram of the ion exchange resin after replacement in Example 3. After being fully rinsed with sodium carbonate solution, the resin can be well regenerated for recycling, and the Li element is finally recovered in the form of lithium carbonate.

[0088] See also Figure 4 , which is the XRD pattern of the Na4Fe3(PO4)2P2O7 material prepared in Example 4. It can be seen that the synthesized material is completely consistent with the standard spectrum, proving the crystal structure and high purity of the product.

[0089] join Figure 5 , which is the charge and discharge curve of the half-cell using the Na4Fe3(PO4)2P2O7 material prepared in Example 4 as the positive electrode material. It can be seen that the prepared positive electrode material has high specific capacity, stable cycle and excellent rate performance.

[0090] The present invention recycles each element in the waste lithium iron phosphate positive electrode material in steps, with a high recovery rate. The remaining recovery liquid after recovery can be added with recovered iron and phosphorus recovery products, supplemented with some carbon sources, and then synthesized into Na4Fe3(PO4)2P2O7 positive electrode material, thereby realizing the green closed-loop recovery of waste LiFePO4 battery positive electrode materials and the high-value conversion of low value-added products. The recycling process of the present invention is simple and easy to implement, with a high element recovery rate, good economic benefits and green environmental protection, and is expected to realize the large-scale recycling of waste lithium iron phosphate battery positive electrode materials.

[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for recycling waste lithium iron phosphate positive electrode materials, characterized in that: The following steps are involved: S1. Processing the waste lithium iron phosphate battery positive electrode sheet to obtain waste positive electrode powder; S2, adding a leaching agent to the waste positive electrode powder, wet ball milling and leaching to recover the Fe element to obtain precipitated iron oxide, and adding a precipitating agent to the filtrate to recover part of the P element to obtain iron phosphate; S3, the remaining solution of step S2 is used to recover the Li element through a sodium type ion exchange resin; S4, measuring the Na and P element contents of the residual solution after the replacement recovery in step S3 by ICP, adding a carbon source, and recovering the obtained iron oxide and / or iron phosphate, so that the final molar ratio of Na:Fe:P in the suspension is 4:3:4, and spray drying to obtain a Na4Fe3(PO4)2P2O7 precursor; S5. The precursor is calcined under the protection of an inert atmosphere to obtain Na4Fe3(PO4)2P2O7 positive electrode material.

2. The method for recycling waste lithium iron phosphate positive electrode materials according to claim 1, characterized in that: The step S1 specifically includes: heat-treating the waste lithium iron phosphate battery positive electrode sheet, stripping it from the current collector to obtain the waste positive electrode material, and further calcining and crushing the waste positive electrode material to obtain the waste positive electrode powder.

3. The method for recycling waste lithium iron phosphate positive electrode materials according to claim 1, characterized in that: In step S2, the leaching solution is oxalic acid, and the molar ratio of the waste positive electrode powder to the oxalic acid is 1:

1.

4. The method for recycling waste lithium iron phosphate positive electrode materials according to claim 1, characterized in that: The leaching time after wet ball milling is 1 to 4 hours.

5. The method for recycling waste lithium iron phosphate positive electrode materials according to claim 1, characterized in that: The precipitant is aqueous ammonia.

6. The method for recycling waste lithium iron phosphate positive electrode materials according to claim 1, characterized in that: The step S3 also includes adding sodium carbonate solution to the replaced ion exchange resin for regeneration to obtain lithium carbonate.

7. The method for recycling waste lithium iron phosphate positive electrode materials according to claim 1, characterized in that: The carbon source is one of citric acid and oxalic acid or a mixture of the two.

8. The method for recycling waste lithium iron phosphate positive electrode materials according to claim 1, characterized in that: In step S4, when only iron oxide is added, another phosphorus source is also added, and the phosphorus source is ammonium dihydrogen phosphate.

9. The method for recycling waste lithium iron phosphate positive electrode materials according to claim 1, characterized in that: In step S4, the spray drying feed rate is 6%, the air intake is 80%, and the spray pyrolysis temperature is 110°C.

10. The method for recycling waste lithium iron phosphate positive electrode materials according to claim 1, characterized in that: In step S5, the inert atmosphere is argon, hydrogen or a mixture of the two.