Hollow cobalt sulfide material, preparation method thereof and application of hollow cobalt sulfide material as adsorbent

Hollow cobalt sulfide materials prepared by the solvothermal method solve the problems of low adsorption capacity and poor selectivity of existing adsorbents in boron separation in salt lake brine, and achieve efficient and stable boron adsorption effect.

CN119018940APending Publication Date: 2024-11-26QINGHAI INST OF SALT LAKES OF CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411236097.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-26

Smart Images

  • Figure CN119018940A_ABST
    Figure CN119018940A_ABST
Patent Text Reader

Abstract

The invention provides a hollow cobalt sulfide material, a preparation method thereof and application of the hollow cobalt sulfide material as an adsorbent, and the hollow cobalt sulfide material is prepared by the following steps: step 1, dispersing a cobalt source and an organic ligand dimethylimidazole in a methanol solution respectively, uniformly mixing, aging, centrifugally separating a solid product, washing and drying to obtain a ZIF-67 precursor; and step 2, dispersing the ZIF-67 precursor obtained in the step 1 and thioacetamide in an ethanol solution, uniformly mixing, carrying out solvothermal reaction, centrifuging the obtained product, washing and drying to obtain the hollow cobalt sulfide material. The hollow cobalt sulfide material is used for adsorption separation of boron in salt lake brine for the first time. And the adsorbent shows excellent boron adsorption performance in a Rogou measure and a Qarhan salt lake.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical adsorption, and in particular to a hollow cobalt sulfide material and a preparation method thereof and application thereof as an adsorbent. Background Art

[0002] Currently, the commonly used methods for extracting boron from aqueous solutions include electrocoagulation, precipitation, membrane separation, ion exchange and adsorption.

[0003] Electrocoagulation technology uses electrochemical principles to use aluminum, iron and other alloy metals as the main electrodes. It uses external pulsed high voltage to produce electrochemical reactions, converts electrical energy into chemical energy, and produces metal cation flocculants at the expense of anode metal electrodes. It separates pollutants from water bodies through coagulation, flotation, reduction and oxidation decomposition, thereby achieving water purification.

[0004] The principle of precipitation method for removing boron is to use a precipitant to convert the boron in the solution into an insoluble borate precipitate or low-solubility boric acid. This method can be divided into alkali precipitation method and acid precipitation method. In alkali precipitation method, the boron in the solution reacts with metal oxides under weak alkaline conditions to form an insoluble borate precipitate; the main principle of acid precipitation method is to use the low solubility of boric acid in inorganic acid to separate crude boric acid by adding hydrochloric acid or sulfuric acid to form a boric acid precipitate.

[0005] Membrane separation uses a selective semipermeable membrane as the separation medium. By applying a driving force (such as concentration difference, pressure difference, potential difference, etc.) on both sides of the membrane, the raw material components selectively pass through the semipermeable membrane, thereby achieving the purpose of separation. It includes reverse osmosis, forward osmosis, nanofiltration and electrodialysis. Among them, the most widely used is the reverse osmosis method, the principle of which is to apply external force on the side with higher concentration, and penetrate into the low concentration area through the selective permeability of the semipermeable membrane, thereby separating boron from the aqueous solution.

[0006] Ion exchange resin is made by introducing different types of functional active groups into a three-dimensional network structure. The principle of boron removal is the complexation reaction between the polyhydroxyl functional groups and the tetrahydroxyborate ion [B(OH)4] (the alkaline polyhydroxyl functional groups and [B(OH)4] - The purpose of boron removal is achieved by complexing with boron or complexing with acidic polyhydroxy functional groups and H3BO3) and the adsorption of boron by resin.

[0007] The adsorption method has the advantages of complete boron removal, simple process, and recyclable adsorption materials, making it the most promising separation method. Boron is an electron-deficient atom that easily forms multi-center bonds. The adsorption method utilizes the electron-deficient characteristics of boron and its easy adsorption by adsorbents to remove boron from the solution by adsorbing on the surface of the adsorbent.

[0008] The design of adsorbent is the key to the adsorption process. Common boron adsorbents include polyhydroxy polymers (methylglucamine, mannitol, sorbitol; adsorption capacity of 5.9-7.2 mg / g), chelating resins (2.648 mg / g), oxides and hydroxides (MgO, Mg(OH)2; adsorption capacity of 13.14, 87 mg / g), clays and layered double hydroxides (Mg-Al-CLDHs, Ca-Al-CLDHs, Zn-Al-CLDHs; adsorption capacity of 35, 11.2, 77.8 mg / g), and magnetic-based adsorbents (MgFe2O4, GO-Fe3O4; adsorption capacity of 68.9, 35.7 mg / g). However, these adsorbents are usually accompanied by low adsorption capacity, poor selectivity, low regeneration efficiency, and secondary pollution, which greatly limits the efficient separation of boron.

[0009] Boron is mainly distributed in the earth's lithosphere and hydrosphere in nature. In the hydrosphere, the most abundant boron resources are in salt lakes. However, during the development process, borates are not precipitated in the form of crystalline salts. In addition, trace amounts of boron remaining from incomplete deboration of old brine in salt lakes directly affect the production of high-quality magnesium and lithium products downstream. Therefore, separating and recovering boron from salt lake brine is an important way to meet the growing demand for boron. Summary of the invention

[0010] The purpose of the present invention is to provide a hollow cobalt sulfide material and a preparation method thereof in view of the technical defects existing in the prior art.

[0011] Another object of the present invention is to provide the use of the hollow cobalt sulfide material as an adsorbent in the adsorption and separation of boron in salt lake brine.

[0012] The technical solution adopted to achieve the purpose of the present invention is:

[0013] A method for preparing a hollow cobalt sulfide material comprises the following steps:

[0014] Step 1, dispersing the cobalt source and the organic ligand dimethylimidazole in a methanol solution respectively, mixing them evenly and then aging them, centrifuging and separating the solid product, washing and drying them to obtain a ZIF-67 precursor;

[0015] Step 2, dispersing the ZIF-67 precursor and thioacetamide obtained in step 1 in an ethanol solution respectively, mixing them evenly, and then performing a solvent thermal reaction. The obtained product is centrifuged, washed, and dried to obtain a hollow cobalt sulfide material.

[0016] In the above technical scheme, in step 1, the cobalt source is cobalt nitrate hexahydrate, cobalt chloride or cobalt sulfate. When the cobalt source is cobalt nitrate hexahydrate, the mass ratio of cobalt nitrate hexahydrate to dimethylimidazole is (1.1-1.5):(2.1-2.5); when the cobalt source is cobalt chloride, the mass ratio of cobalt chloride to dimethylimidazole is (0.21-0.25):(1.3-1.7); when the cobalt source is cobalt sulfate, the mass ratio of cobalt sulfate to dimethylimidazole is (0.25-0.31):(1.5-1.8).

[0017] In the above technical solution, in step 1, the aging time is 6-24 hours.

[0018] In the above technical solution, in step 1, the drying temperature is 60-120° C., and the drying time is 10-12 hours.

[0019] In the above technical solution, in step 2, the mass ratio of ZIF-67 precursor to thioacetamide is (0.05-0.15): (0.05-0.25).

[0020] In the above technical solution, in step 2, the solvent thermal reaction is carried out in a high-pressure reactor with a polytetrafluoroethylene lining.

[0021] In the above technical solution, in step 2, the reaction temperature of the solvent thermal reaction is 80-140° C., and the reaction time is 2-6 hours.

[0022] In the above technical solution, in step 2, the drying temperature is 60-120° C., and the drying time is 10-12 hours.

[0023] Another aspect of the present invention also includes a hollow cobalt sulfide material prepared according to the preparation method, wherein the hollow cobalt sulfide material is a polycrystalline material, the hollow cobalt sulfide material is a dodecahedral structure with a smooth surface and a hollow structure inside, and the shell thickness of the hollow cobalt sulfide material is 13 to 15 nm.

[0024] Another aspect of the present invention also includes the use of the hollow cobalt sulfide material as an adsorbent in the adsorption and separation of boron in salt lake brine.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. The present invention adopts a solvothermal method and thioacetamide as a vulcanizing agent to prepare a hollow cobalt sulfide material derived from ZIF-67. The preparation method is simple, and the construction of the hollow structure can adjust the pore volume, thereby providing abundant adsorption sites and achieving high adsorption capacity. In this application, thioacetamide is selected as a vulcanizing agent, and the surface of the obtained hollow cobalt sulfide material is a smooth structure. When other vulcanizing agents are selected, the surface of the obtained hollow cobalt sulfide material is a nano-sheet structure, which affects the adsorption performance.

[0027] 2. The hollow cobalt sulfide material of the present invention is used for the first time to adsorb and separate boron from salt lake brine. It exhibits excellent boron adsorption performance in Lagocuo and Chaerhan salt lakes, with adsorption capacities of 162 mg / g and 92 mg / g, respectively. The adsorption capacity in a boron-containing aqueous solution is 253.15 mg / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 (a) is the XRD pattern of the ZIF-67 precursor, and (b) is the XRD pattern of the hollow cobalt sulfide material.

[0029] Figure 2 TEM, HRTEM and thickness images of ZIF-67 precursor and hollow cobalt sulfide material, where (a) is a scanning electron microscope image of ZIF-67 precursor, (b) and (c) are transmission electron microscope images of hollow cobalt sulfide material, (d) is a thickness measurement image of hollow cobalt sulfide material, (e) is a high-magnification transmission electron microscope image of hollow cobalt sulfide material, and (f) is a selected area electron diffraction image of hollow cobalt sulfide material.

[0030] Figure 3 Activity diagram of boron adsorption of ZIF-67 precursor and hollow cobalt sulfide material in boron-containing aqueous solution.

[0031] Figure 4 This is the activity diagram of hollow cobalt sulfide materials in adsorbing boron in the original brine of Lagocuo and Chaerhan Salt Lakes.

[0032] Figure 5 (a) shows the selectivity of hollow cobalt sulfide materials, and (b) is a schematic diagram of the cyclic stability of hollow cobalt sulfide materials. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0034] Example 1

[0035] A method for preparing a hollow cobalt sulfide material comprises the following steps:

[0036] Step 1: Cobalt nitrate hexahydrate is used as a cobalt source and dimethylimidazole is used as an organic ligand, which are dispersed in 20 ml of methanol solution, wherein the mass of cobalt nitrate hexahydrate is 1.1 g and the mass of dimethylimidazole is 2.2 g, and stirred at room temperature for 30 min, and then the two solutions are mixed and stirred continuously at room temperature for 20 min. The mixed solution is aged for 12 h, the obtained product is centrifuged, washed several times with a methanol solution, and dried at 60 ° C for 10 h to obtain a ZIF-67 precursor.

[0037] Step 2, disperse the ZIF-67 precursor and thioacetamide in an ethanol solution, wherein the mass of the ZIF-67 precursor is 0.09g, the mass of the thioacetamide is 0.17g, the amount of ethanol added is 30ml, and the mixture is stirred at room temperature for 20min. The above mixed solution is poured into a high-pressure reactor equipped with a polytetrafluoroethylene liner, heated to react at a reaction temperature of 100°C and a reaction time of 3h. The obtained product is centrifuged, washed several times with deionized water and anhydrous ethanol, respectively, and dried at 60°C for 10h to obtain a hollow cobalt sulfide material, recorded as Co3S4-H.

[0038] The hollow cobalt sulfide material obtained in Example 1 was characterized. Figure 1 As shown, ZIF-67 shows no impurity peaks when compared with the simulated standard card, and the diffraction peaks of the hollow structure cobalt sulfide material match the standard card (JCPDS No.00-047-1738).

[0039] Depend on Figure 2 (a) shows that the ZIF-67 precursor is a dodecahedral structure. Figure 2 As can be seen from (b) and (c) in the figure, the hollow cobalt sulfide material is a hollow structure with a smooth surface. Figure 2 (d) shows that the shell thickness of the hollow cobalt sulfide material is 14.08 nanometers. Figure 2 As can be seen in (e), the lattice spacing of the hollow cobalt sulfide material is 0.166 and 0.285 nm, corresponding to the (4 4 0) and (3 1 1) crystal planes of the standard card, respectively. Figure 2 As can be seen from (f) in the figure, the hollow cobalt sulfide material is a polycrystalline material, and the concentric circle radii r1=0.281 and r2=0.167, corresponding to the (3 1 1) and (4 4 0) crystal planes, respectively.

[0040] Example 2

[0041] A method for preparing a hollow cobalt sulfide material comprises the following steps:

[0042] Step 1: Cobalt nitrate hexahydrate is used as a cobalt source and dimethylimidazole is used as an organic ligand. They are dispersed in 15 ml of methanol solution, wherein the mass of cobalt nitrate hexahydrate is 1.4 g and the mass of dimethylimidazole is 2.4 g. Stir at room temperature for 50 min, then mix the two solutions, and continue stirring at room temperature for 50 min. The mixed solution is aged for 18 h, the resulting product is centrifuged, washed several times with a methanol solution, and dried at 60 ° C for 12 h to obtain a ZIF-67 precursor.

[0043] Step 2, disperse the ZIF-67 precursor and thioacetamide in an ethanol solution, wherein the mass of the ZIF-67 precursor is 0.1g, the mass of the thioacetamide is 0.15g, the amount of ethanol added is 40ml, and the mixture is stirred at room temperature for 10min. The above mixed solution is poured into a high-pressure reactor equipped with a polytetrafluoroethylene liner, heated to react at a reaction temperature of 110°C and a reaction time of 3h. The obtained product is centrifuged, washed several times with deionized water and anhydrous ethanol, dried at 60°C for 12h, and a hollow cobalt sulfide material is obtained, recorded as Co3S4-H.

[0044] Example 3

[0045] A method for preparing a hollow cobalt sulfide material comprises the following steps:

[0046] Step 1: Cobalt nitrate hexahydrate is used as a cobalt source and dimethylimidazole is used as an organic ligand, which are dispersed in 10-30 ml of methanol solution, wherein the mass of cobalt nitrate hexahydrate is 1.45 g and the mass of dimethylimidazole is 2.18 g, and stirred at room temperature for 30 minutes. The two solutions are then mixed and stirred for 40 minutes at room temperature. The mixed solution is aged for 20 hours, the obtained product is centrifuged, washed several times with a methanol solution, and dried at 60°C for 12 hours to obtain a ZIF-67 precursor.

[0047] Step 2, disperse the ZIF-67 precursor and thioacetamide in an ethanol solution, wherein the mass of the ZIF-67 precursor is 0.12g, the mass of the thioacetamide is 0.11g, the amount of ethanol added is 50ml, and the mixture is stirred at room temperature for 20min. The above mixed solution is poured into a high-pressure reactor equipped with a polytetrafluoroethylene liner, heated to react at a reaction temperature of 130°C and a reaction time of 4h. The obtained product is centrifuged, washed several times with deionized water and anhydrous ethanol, dried at 60°C for 10h, and a hollow cobalt sulfide material is obtained, recorded as Co3S4-H.

[0048] Example 4

[0049] The hollow cobalt sulfide material obtained in Example 1 was used as an adsorbent to verify its boron adsorption activity in a boron-containing aqueous solution (200 mg / l boric acid aqueous solution). Figure 3 As shown, compared with the ZIF-67 precursor, the hollow cobalt sulfide material has higher boron adsorption performance, with an adsorption capacity of 283.3 mg / g.

[0050] Example 5

[0051] The hollow cobalt sulfide material obtained in Example 1 was used as an adsorbent to verify its activity in adsorbing boron in the raw brine of Laguocuo and Chaerhan Salt Lakes. Figure 4 As shown, hollow cobalt sulfide has a high boron adsorption capacity in salt lake brine, with a boron adsorption capacity of 167 mg / g in Lagocuo Salt Lake and 92 mg / g in Chaerhan Salt Lake. From the selectivity results, it can be seen that Co3S4-H is negatively charged and attracts cations during the adsorption process to form a cation layer, which hinders the combination of Co3S4-H and H3BO3. In addition, studies have shown that the smaller the radius of the cation, the stronger the double layer structure and the greater the resistance to the adsorbate. K in Chaerhan Salt Lake + The concentration is much greater than that of Lagocuo Salt Lake, and the ion radius K + >Ca 2+ >Mg 2+ Therefore, the boron adsorption capacity of Lagocuo Salt Lake is greater than that of Qarhan Salt Lake.

[0052] The hollow cobalt sulfide material obtained in Example 2-3 was used as an adsorbent, and exhibited an adsorption activity similar to that of the hollow cobalt sulfide material in Example 1.

[0053] Example 6

[0054] The hollow cobalt sulfide material obtained in Example 1 was used as an adsorbent to verify its selectivity and cycle stability.

[0055] like Figure 5 As shown in Figure 2, under the interference of anions, the adsorption capacity of Co3S4-H is more selective, and the adsorption capacity decreases by 1.3%, 0.38% and 2.5%, respectively. Under the interference of cations (such as Figure 5 As shown in (a), the B adsorption capacity of Co3S4-H decreased by 34%, 41.9% and 44.1%, respectively. However, B in salt lake brine mainly exists in the form of boric acid molecules or borate anions. 2+ Mg 2+ and K + The ions have an effect on the adsorption of B, but the boric acid adsorption capacities are 715.08, 632.48, and 608.8 mg / g, respectively, which further confirms that the Co3S4-H material has a higher adsorption capacity for B. The separation factor and adsorption separation coefficient after adsorption are shown in Table 1.

[0056] Table 1

[0057]

[0058] As can be seen from Table 1, the distribution coefficient of B is much greater than that of Ca 2+ Mg 2+ and K + , indicating that Co3S4-H material is more inclined to the adsorption of B, while Ca 2+ and Mg 2+ The separation factor is greater than 100, indicating that compared with K + , Ca 2+ and Mg 2+ The two ions have little effect on the adsorption of B. In addition, it can be seen from Table 1 that although the introduction of cations affects the adsorption of B, the adsorption of Ca 2+ Mg 2+ and K + The concentration of H3BO3 did not change. This may be attributed to the double layer principle. Co3S4-H is negatively charged and attracts cations during adsorption, forming a cation layer, which hinders the combination of Co3S4-H and H3BO3. In addition, studies have shown that the smaller the radius of the cation, the stronger the double layer structure and the greater the resistance to the adsorbate. The results of the cycle experiment show that ( Figure 5 b) The adsorption capacity decreased significantly during the five adsorption-desorption experiments. Compared with the first adsorption-desorption experiment, the adsorption capacity decreased by 2.8%, 10.4%, 18.6% and 19.4% respectively. The adsorption capacity of the last cycle reached 80% of that of the first cycle.

[0059] The above is only a preferred embodiment of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a hollow cobalt sulfide material, characterized in that: The following steps are involved: Step 1, dispersing the cobalt source and the organic ligand dimethylimidazole in a methanol solution respectively, mixing them evenly and then aging them, centrifuging and separating the solid product, washing and drying them to obtain a ZIF-67 precursor; Step 2, dispersing the ZIF-67 precursor and thioacetamide obtained in step 1 in an ethanol solution respectively, mixing them evenly, and then performing a solvent thermal reaction. The obtained product is centrifuged, washed, and dried to obtain a hollow cobalt sulfide material.

2. The preparation method according to claim 1, characterized in that: In the step 1, the cobalt source is cobalt nitrate hexahydrate, cobalt chloride or cobalt sulfate. When the cobalt source is cobalt nitrate hexahydrate, the mass ratio of cobalt nitrate hexahydrate to dimethylimidazole is (1.1-1.5):(2.1-2.5); when the cobalt source is cobalt chloride, the mass ratio of cobalt chloride to dimethylimidazole is (0.21-0.25):(1.3-1.7); when the cobalt source is cobalt sulfate, the mass ratio of cobalt sulfate to dimethylimidazole is (0.25-0.31):(1.5-1.8).

3. The preparation method according to claim 1, characterized in that: In the step 1, the aging time is 6-24 hours.

4. The preparation method according to claim 1, characterized in that: In the step 1, the drying temperature is 60-120° C. and the drying time is 10-12 hours.

5. The preparation method according to claim 1, characterized in that: In the step 2, the mass ratio of the ZIF-67 precursor to thioacetamide is (0.05-0.15): (0.05-0.25).

6. The preparation method according to claim 1, characterized in that: In the step 2, the solvent thermal reaction is carried out in a high-pressure reactor with a polytetrafluoroethylene liner.

7. The preparation method according to claim 1, characterized in that: In the step 2, the reaction temperature of the solvent thermal reaction is 80-140° C., and the reaction time is 2-6 hours.

8. The preparation method according to claim 1, characterized in that: In the step 2, the drying temperature is 60-120° C. and the drying time is 10-12 hours.

9. The hollow cobalt sulfide material prepared according to the preparation method according to any one of claims 1 to 8, characterized in that: The hollow cobalt sulfide material is a polycrystalline material, and the hollow cobalt sulfide material is a dodecahedral structure with a smooth surface and a hollow structure inside. The shell thickness of the hollow cobalt sulfide material is 13-15 nm.

10. Use of the hollow cobalt sulfide material according to claim 9 as an adsorbent in the adsorption and separation of boron from salt lake brine.