Method for regulating highly exposed (010) crystal face of layered oxide positive electrode material

By introducing aluminum nitrogen compounds and silicon-containing compounds into the precursor of the layered oxide positive electrode material, the solid phase method is used to induce (010) crystal surface excellent growth and doping modification, the cost and complex process in the prior art is solved. Problem, the industrial production of high-performance layered oxide cathode materials has been achieved.

CN119018944AActive Publication Date: 2024-11-26ZHENGZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411200923.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-26
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The prior art is difficult to achieve high exposure (010) crystal plane of layered oxide cathode material at low cost, resulting in insufficient rate performance and cycle stability, and complex processes and unsuitable for large-scale industrial production.

Method used

The aluminum nitrogen compound and silicon-containing compound modified material are introduced into the layered oxide positive electrode material precursor. The crystal surface is induced (010) during the sintering process by a simple solid phase method, and doping and coating modification are carried out. , adjust process parameters to improve material performance.

Benefits of technology

The rate performance improvement and specific capacity and cycle stability of the layered oxide cathode material with high exposure (010) crystal surface are achieved. The method is simple, versatile, and low-cost, and is suitable for industrial production applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion battery electrode materials, and particularly relates to a method for regulating and controlling a highly exposed (010) crystal face of a layered oxide positive electrode material. An aluminum-nitrogen compound and a silicon-containing compound modified material are introduced into a layered oxide positive electrode precursor by adopting a solid phase method, layered oxide material crystals are induced to preferentially grow along the (010) crystal face by utilizing the modified material in the subsequent sintering lithiation process, and finally the layered oxide positive electrode material with the highly exposed (010) crystal face is obtained. The layered oxide positive electrode material with the highly-exposed (010) crystal face is good in primary grain uniformity and high in structural stability, the rate capability of the layered oxide positive electrode material is improved, meanwhile, the material is subjected to doping and coating modification, and the specific capacity and the cycling stability are remarkably improved; the method is simple in process, high in universality, low in cost and outstanding in performance, and has great industrial production and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion battery electrode materials, and in particular relates to a method for regulating a layered oxide positive electrode material to have a highly exposed (010) crystal plane. Background Art

[0002] The rapid development of electric vehicles and electric aircraft has put forward higher requirements on the power density of lithium-ion batteries. Layered oxide cathode materials have higher discharge specific capacity and discharge voltage, and are currently the preferred materials for high energy density lithium-ion power batteries. However, layered oxide cathode materials still cannot meet the high power requirements of lithium-ion power batteries in terms of rate performance.

[0003] In layered oxide materials, the (010) plane along the c-axis direction has a completely open characteristic, which is the Li + The exposed (010) surface can ensure the active crystal surface of Li + The deintercalation process is smooth. Existing technologies usually use the regulation of the morphological structure of the precursor and the doping of the precursor elements to achieve this. The precursor morphology is adjusted by regulating the reaction time, reaction pH, ammonia concentration and other process parameters during the co-precipitation reaction, and then the layered positive electrode material is used to inherit the characteristics of the precursor morphology to induce the exposure of the (010) crystal plane, and a layered oxide positive electrode material with a high exposure (010) crystal plane can be obtained. In addition, the formation energy of the (010) crystal plane can also be reduced by doping with precursor elements, which promotes the exposure of the (010) crystal plane during the lithiation process.

[0004] However, these technical processes are complex and have extremely stringent requirements on the preparation conditions of the precursors, making them difficult to implement in industrialization. For example, the Chinese patent with publication number CN115849460A discloses a preparation method for regulating the preferential growth of the (010) crystal plane of a ternary material, wherein a layered oxide precursor material is doped with tungsten, and a tungsten-doped layered oxide positive electrode material with a high (010) exposure surface is prepared by adjusting the addition method of the tungsten source and the lithiation sintering method, thereby effectively improving the electrochemical performance of the material. However, the special tungsten source addition method and the lithiation sintering method in this patent have complex process conditions, which greatly increases the production cost and is not conducive to industrial large-scale production.

[0005] Based on this, the present invention adopts a simple solid phase method, without changing the original precursor and the lithiation sintering process, and only introduces aluminum nitrogen compounds and silicon-containing compound modification materials into the layered oxide positive electrode precursor, so that the modified materials can be used to induce the layered oxide material crystals to grow preferentially along the (010) crystal plane during the subsequent sintering and lithiation process. In addition, while inducing the preferential growth of the (010) crystal plane, the present invention also achieves doping and coating modification of the material, thereby achieving simultaneous improvement of the rate performance, specific capacity and cycle life of the layered oxide positive electrode material. The preparation method of the present invention has extremely strong versatility and can be applied to layered oxide single crystals and polycrystalline positive electrode materials with various nickel contents. Summary of the invention

[0006] The purpose of the present invention is to propose a method for regulating the high exposure (010) crystal plane of layered oxide positive electrode materials, in view of the problem that the existing technology is difficult to achieve high exposure (010) crystal planes of layered oxide positive electrode materials at low cost. The method only introduces modified materials into the precursor through a simple solid-phase method and adjusts the preparation process parameters. Not only the rate performance of layered oxide positive electrode materials with high exposure (010) crystal planes is improved, but also the material is doped and coated to significantly improve the specific capacity and cycle stability. The method is simple in process, strong in versatility, low in cost, and has outstanding performance, and has great prospects for industrial production and application.

[0007] Furthermore, the present invention also provides the use of the layered oxide positive electrode material with a high exposure (010) crystal plane prepared by the method in the preparation of lithium-ion batteries.

[0008] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:

[0009] A method for preparing a layered oxide positive electrode material with a highly exposed (010) crystal plane comprises the following steps:

[0010] The layered oxide positive electrode material precursor, lithium source, aluminum nitrogen compound and silicon-containing compound are uniformly mixed in a certain molar ratio, and then placed in an atmosphere furnace for sintering to obtain a layered oxide positive electrode material with a highly exposed (010) crystal plane.

[0011] Furthermore, the chemical formula of the layered oxide positive electrode material precursor is Ni 1-x-y-z Co x Mn y Al z (OH)2, x≥0, y≥0, z≥0, 0.3<(1-xyz)≤1.

[0012] More preferably, the chemical formula of the layered oxide positive electrode material precursor is Ni 0.96 Co 0.015Mn 0.015 Al 0.01 (OH)2、Ni 0.83 Co 0.12 Mn 0.05 (OH)2.

[0013] Furthermore, the lithium source is one or more of lithium hydroxide, lithium carbonate and lithium nitrate.

[0014] Furthermore, the aluminum nitrogen compound is a combination of one or more of dihydroxyamino aluminum acetate, aluminum nitride, and aluminum nitrate.

[0015] Furthermore, the silicon-containing compound is a combination of one or more of silicon dioxide, silicon nitride, silicon hexaboride, silicon carbide, lithium silicate, and silicon tetrafluoride.

[0016] Furthermore, the molar ratio of the layered oxide positive electrode material precursor, the lithium source, the aluminum nitrogen compound and the silicon-containing compound is 1:(0.9-1.6):(0.0001-1):(0.0001-1).

[0017] Furthermore, the atmosphere in the atmosphere furnace is an oxygen atmosphere, a nitrogen atmosphere, an ammonia atmosphere, a sulfur dioxide atmosphere, a hydrogen sulfide atmosphere, or a combination of any two of these five gases.

[0018] Furthermore, the sintering includes one-stage sintering and two-stage sintering; the temperature of the one-stage sintering is 200-650°C; the time of the one-stage sintering is 0.5-24h; the temperature of the two-stage sintering is 500-1300°C; the time of the two-stage sintering is 1-72h.

[0019] Furthermore, the present invention also provides a layered oxide positive electrode material with a high exposure (010) crystal plane prepared by the above method, which has good rate performance, specific capacity and cycle stability and can be used to prepare lithium-ion batteries.

[0020] Furthermore, based on a general inventive concept, the present invention also provides the use of the layered oxide positive electrode material with a high exposure of (010) crystal plane in the preparation of a lithium-ion battery.

[0021] Furthermore, the present invention also provides a method for preparing a lithium-ion battery using the layered oxide positive electrode material with a high exposure (010) crystal plane, which specifically comprises the following steps:

[0022] a. placing a certain amount of a layered oxide cathode material having a highly exposed (010) crystal plane, a conductive agent and a binder in a container to obtain a mixed powder;

[0023] b. Add a solvent to the mixed powder in step a, ultrasonically disperse it at a power of 80 to 100 W for 8 to 12 minutes, then place a polytetrafluoroethylene magnet in a container and stir it at a speed of 300 to 400 r / min for 8 to 12 hours to evenly disperse the layered oxide positive electrode material and the conductive agent with a high exposure (010) crystal plane to obtain a mixed slurry;

[0024] c. Coat the mixed slurry in step b on aluminum foil (current collector), dry it at 60-80°C for 8-12h, and then make it into a button-type electrode sheet; then use the prepared electrode sheet as the working electrode, the metal lithium sheet as the counter electrode, install a diaphragm, and use a high-nickel 4.3V electrolyte to assemble a button battery. The battery model is a CR2032 button battery.

[0025] Specifically, in step a, the conductive agent is carbon black (Super-P); and the binder is PVDF.

[0026] Specifically, the solvent is selected from one of deionized water, ethanol and NMP.

[0027] Specifically, the mass of the solvent is 1 to 1.5 times the mass of the mixed powder.

[0028] Specifically, in the mixed slurry obtained in step b, the weight ratio of the layered oxide positive electrode material with a highly exposed (010) crystal plane, the conductive agent, and the binder is (16-18):1:(1-2).

[0029] Specifically, the diaphragm type is a polypropylene diaphragm, and the main component of the electrolyte used in the battery is: lithium salt (lithium hexafluorophosphate); preferably, the electrolyte is 1M LiPF6 in EC:EMC=3:7Vol%, with 2wt% vinylene carbonate VC additive added.

[0030] Specifically, in step c, the loading amount of the mixed slurry on the prepared electrode sheet is 1 to 20 mg / cm 2 .

[0031] Furthermore, based on a general inventive concept, the present invention also provides a lithium-ion battery prepared using the layered oxide positive electrode material with a high exposure of (010) crystal planes.

[0032] Compared with the prior art, the advantages of the present invention are:

[0033] 1. The present invention adopts a solid phase method, and only introduces the modified material in the process of mixing the precursor into the lithium source, inducing the layered oxide positive electrode material to highly expose the (010) crystal plane. The method is simple and does not change the existing industrial production process, and can be quickly promoted on a large scale.

[0034] 2. The preparation method for regulating the highly exposed (010) crystal plane of the layered oxide positive electrode material of the present invention has extremely strong versatility and is applicable to layered oxide single crystal and polycrystalline positive electrode materials with various nickel contents, and the prepared materials have good uniformity.

[0035] 3. While regulating the rate performance of the layered oxide positive electrode material with a high exposure (010) crystal plane, the present invention also dopes aluminum, nitrogen and silicon elements into the layered oxide positive electrode material, and forms a coating layer of aluminum oxide and silicon oxide, thereby achieving doping and coating modification of the material, further improving the specific capacity and cycle stability of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 LiNi prepared in Comparative Example 1 0.96 Co 0.015 Mn 0.015 Al 0.01 SEM image of O2;

[0037] Figure 2 LiNi prepared in Comparative Example 2 0.83 Co 0.12 Mn 0.05 SEM image of O2;

[0038] Figure 3 The LiNi with highly exposed (010) crystal plane prepared in Example 1 0.96 Co 0.015 Mn 0.015 Al 0.01 SEM image of O2;

[0039] Figure 4 The LiNi with highly exposed (010) crystal plane prepared in Example 2 0.83 Co 0.12 Mn 0.05 SEM image of O2;

[0040] Figure 5 It is the rate performance diagram of comparative example 1 and embodiment 1;

[0041] Figure 6 It is the cycle performance diagram of comparative example 1 and example 1 at 0.5C rate;

[0042] Figure 7 It is the rate performance diagram of comparative example 2 and embodiment 2;

[0043] Figure 8 It is the cycle performance diagram of comparative example 2 and example 2 at 1C rate. DETAILED DESCRIPTION

[0044] The following examples will further illustrate the present invention in conjunction with the accompanying drawings. This embodiment is implemented based on the technical solution of the present invention, and provides detailed implementation methods and processes, but the protection scope of the present invention is not limited to the following embodiments.

[0045] The experimental methods in the following examples without specifying specific conditions are generally carried out under conventional conditions, and the raw materials and reagents used are conventional commercially available products unless otherwise specified.

[0046] The comparative examples and examples all use Ni provided by Henan Xinxiang Tianli Lithium Energy Co., Ltd. 0.96 Co 0.015 Mn 0.015 Al 0.01 (OH)2、Ni 0.83 Co 0.12 Mn 0.05 The (OH)2 layered oxide positive electrode material precursor is used as the raw material, and its preparation method can adopt the conventional method in the prior art, and it is not the inventive point of the present invention, so it will not be repeated.

[0047] Comparative Example 1

[0048] Ni 0.96 Co 0.015 Mn 0.015 Al 0.01 The (OH)2 layered oxide cathode material precursor and LiOH·H2O were uniformly mixed in a molar ratio of 1:1.03, and then placed in an oxygen atmosphere furnace for two-stage sintering. The first stage sintering temperature was 400°C, the sintering time was 4h, and the second stage sintering temperature was 720°C, the sintering time was 10h, and the layered oxide cathode material LiNi was obtained. 0.96 Co 0.015 Mn 0.015 Al 0.01 O2.

[0049] The layered oxide positive electrode material LiNi obtained in Comparative Example 1 0.96 Co 0.015 Mn 0.015 Al 0.01 The SEM image of O2 is as follows Figure 1 As shown, from Figure 1 It can be seen that the layered oxide positive electrode material LiNi 0.96 Co 0.015 Mn 0.015 Al 0.01 The secondary particles of O2 are spherical with a size of 10 μm, and the primary particles are irregular grains.

[0050] Comparative Example 2

[0051] Ni 0.83 Co0.12 Mn 0.05 The (OH)2 layered oxide cathode material precursor and LiOH·H2O were uniformly mixed in a molar ratio of 1:1.03, and then placed in an oxygen atmosphere furnace for two-stage sintering. The first stage sintering temperature was 500°C, the sintering time was 6h, and the second stage sintering temperature was 780°C, the sintering time was 12h, and the layered oxide cathode material LiNi was obtained. 0.83 Co 0.12 Mn 0.05 O2.

[0052] Comparative Example 2 obtained layered oxide positive electrode material LiNi 0.83 Co 0.12 Mn 0.05 The SEM image of O2 is as follows Figure 2 As shown, from Figure 2 It can be seen that the layered oxide positive electrode material LiNi 0.83 Co 0.12 Mn 0.05 The secondary particles of O2 are spherical with a size of 12 μm, and the primary particles are irregular grains.

[0053] Example 1

[0054] Example 1 provides a method for preparing a layered oxide positive electrode material with a highly exposed (010) crystal plane, the specific steps of which are:

[0055] Ni 0.96 Co 0.015 Mn 0.015 Al 0.01 The (OH)2 layered oxide cathode material precursor, LiOH·H2O, dihydroxyaminoacetic acid aluminum and silicon dioxide were uniformly mixed in a molar ratio of 1:1.03:0.01:0.0065, and then placed in an oxygen atmosphere furnace for two-stage sintering. The first stage sintering temperature was 400°C and the sintering time was 4h. The second stage sintering temperature was 720°C and the sintering time was 10h. The layered oxide cathode material LiNi with a highly exposed (010) crystal plane was obtained. 0.96 Co 0.015 Mn 0.015 Al 0.01 O2.

[0056] Layered oxide positive electrode material LiNi obtained in Example 1 0.96 Co 0.015 Mn 0.015 Al 0.01 The SEM image of O2 is as follows Figure 3 As shown, from Figure 3 It can be seen that the layered oxide positive electrode material LiNi with high exposed (010) crystal plane in Example 1 0.96 Co0.015 Mn 0.015 Al 0.01 The secondary O2 particles are spherical with a size of 10 μm, and the primary particles are long single crystal grains.

[0057] Example 2

[0058] Example 2 provides a method for preparing a layered oxide positive electrode material with a highly exposed (010) crystal plane, the specific steps of which are:

[0059] Ni 0.83 Co 0.12 Mn 0.05 The (OH)2 layered oxide cathode material precursor, LiOH·H2O, dihydroxyaminoacetic acid aluminum and silicon dioxide were uniformly mixed in a molar ratio of 1:1.03:0.01:0.0065, and then placed in an oxygen atmosphere furnace for two-stage sintering. The first stage sintering temperature was 500°C and the sintering time was 6h. The second stage sintering temperature was 780°C and the sintering time was 12h. The layered oxide cathode material LiNi with a highly exposed (010) crystal plane was obtained. 0.83 Co 0.12 Mn 0.05 O2.

[0060] Layered oxide positive electrode material LiNi obtained in Example 2 0.83 Co 0.12 Mn 0.05 The SEM image of O2 is as follows Figure 4 As shown, from Figure 4 It can be seen that the layered oxide positive electrode material LiNi with high exposed (010) crystal plane in Example 2 0.83 Co 0.12 Mn 0.05 The secondary O2 particles are spherical with a size of 12 μm, and the primary particles are long single crystal crystalline grains.

[0061] Performance Testing

[0062] The products prepared in Example 1-2 and Comparative Example 1-2 were used to prepare lithium-ion batteries, and the specific preparation method was as follows:

[0063] a. The active material (layered oxide positive electrode material prepared in Examples 1 and 2 or Comparative Examples 1 and 2) is mixed with carbon black (Super-P, conductive agent, Shenzhen Kejing Zhida Technology Co., Ltd., CAS1333-86-4) and binder PVDF (polyvinylidene fluoride) in a mass ratio of 90:5:5 to obtain a mixed powder;

[0064] b. Then the mixed powder in step a is added to a solvent (N-methylpyrrolidone, NMP) and placed in a mixing container for uniform mixing. The mass of the solvent is 1.5 times the mass of the mixed powder. Then, ultrasonic dispersion is performed at a power of 100 W for 8 minutes. Then, a polytetrafluoroethylene magnet is placed in the mixing container and stirred at a speed of 400 r / min for 10 hours to uniformly disperse the active substance and carbon black (Super-P) to obtain a mixed slurry.

[0065] c. The mixed slurry in step b was coated on aluminum foil and dried at 80 ° C for 12 h to prepare a loading of 5 mg / cm 2 electrode sheet; then in an argon-protected glove box, the prepared electrode sheet was used as the working electrode, the metal lithium sheet was used as the counter electrode, the polypropylene film was used as the diaphragm, the electrolyte was a high-nickel 4.6V electrolyte (1M LiPF6, EC:EMC=3:7Vol%, with 2wt% vinylene carbonate VC additive), a button battery was assembled, the battery model was a CR2032 button battery, and constant current charge and discharge test was performed.

[0066] Comparing the rate performance of Example 1 and Comparative Example 1, the discharge specific capacity was tested at different rates. Figure 5 shown.

[0067] As can be seen from the figure, the discharge capacity of Example 1 at 0.1C is 238mAh / g, which is higher than 220mAh / g of Comparative Example 1. As the rate increases, the discharge capacity of both Example 1 and Comparative Example 1 decreases, but the decrease in Example 1 is much lower than that in Comparative Example 1. At a high rate of 5C, the discharge capacity of Example 1 is still 192mAh / g, while the discharge capacity of Comparative Example 1 is only 153mAh / g. The results show that the preparation method of layered oxide positive electrode material with high exposure (010) crystal plane proposed in the present invention is beneficial to LiNi 0.96 Co 0.015 Mn 0.015 Al 0.01 Improvement of O2 material rate performance.

[0068] Comparing the cycle performance of Example 1 and Comparative Example 1, the cycle performance at 0.5C rate is shown in the figure below: Figure 6 shown.

[0069] As can be seen from the figure, the initial discharge specific capacity of Example 1 is 216 mAh / g, which is higher than 170 mAh / g of Comparative Example 1. The capacity retention rate of Example 1 after 200 cycles is 76%, which is much higher than 38% of Comparative Example 1. The results show that the preparation method of layered oxide positive electrode material with high exposed (010) crystal plane proposed in the present invention is beneficial to LiNi 0.96 Co 0.015 Mn 0.015 Al0.01 Improvement of O2 material cycle performance.

[0070] Comparing the rate performance of Example 2 and Comparative Example 2, the discharge specific capacity was tested at different rates. Figure 7 shown.

[0071] As can be seen from the figure, the discharge capacity of Example 2 at 0.1C is 197mAh / g, which is higher than 196mAh / g of Comparative Example 2. As the rate increases, the discharge capacity of both Example 2 and Comparative Example 2 decreases, but the decrease in Example 2 is lower than that in Comparative Example 2. At a high rate of 5C, the discharge capacity of Example 2 is still 142mAh / g, which is higher than 132mAh / g of Comparative Example 2. The results show that the method for preparing a layered oxide positive electrode material with a high exposed (010) crystal plane proposed in the present invention is beneficial to LiNi 0.83 Co 0.12 Mn 0.05 Improvement of O2 material rate performance.

[0072] Comparing the cycle performance of Example 2 and Comparative Example 2, the cycle performance at 1C rate is shown in the figure below: Figure 8 shown.

[0073] As can be seen from the figure, the initial discharge specific capacity of Example 2 is 179 mAh / g, which is higher than 175 mAh / g of Comparative Example 2. The capacity retention rate of Example 2 after 100 cycles is 98%, which is higher than 94% of Comparative Example 2. The results show that the preparation method of layered oxide positive electrode material with high exposed (010) crystal plane proposed in the present invention is beneficial to LiNi 0.83 Co 0.12 Mn 0.05 Improvement of O2 material cycle performance.

[0074] In summary, the preparation method of regulating the highly exposed (010) crystal plane of the layered oxide positive electrode material described in the present invention is simple and can effectively improve its overall performance. It has the characteristics of low price and good versatility, and is suitable for large-scale industrial promotion and application.

[0075] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a layered oxide positive electrode material with a highly exposed (010) crystal plane, characterized in that: The following steps are involved: The layered oxide positive electrode material precursor, lithium source, aluminum nitrogen compound and silicon-containing compound are uniformly mixed in a certain molar ratio, and then placed in an atmosphere furnace for sintering to obtain a layered oxide positive electrode material with a highly exposed (010) crystal plane.

2. The preparation method according to claim 1, characterized in that The chemical formula of the layered oxide positive electrode material precursor is Ni 1-x-y-z Co x Mn y Al z (OH)2, x≥0, y≥0, z≥0, 0.3<(1-xyz)≤1.

3. The preparation method according to claim 1, characterized in that: The lithium source is one or more of lithium hydroxide, lithium carbonate and lithium nitrate.

4. The preparation method according to claim 1, characterized in that: The aluminum nitrogen compound is a combination of one or more of dihydroxyamino aluminum acetate, aluminum nitride and aluminum nitrate.

5. The preparation method according to claim 1, characterized in that: The silicon-containing compound is a combination of one or more of silicon dioxide, silicon monoxide, silicon nitride, silicon hexaboride, silicon carbide, lithium silicate and silicon tetrafluoride.

6. The preparation method according to claim 1, characterized in that: The molar ratio of the layered oxide positive electrode material precursor, lithium source, aluminum nitrogen compound and silicon-containing compound is 1:(0.9-1.6):(0.0001-1):(0.0001-1).

7. The preparation method according to claim 1, characterized in that: The atmosphere in the atmosphere furnace is an oxygen atmosphere, a nitrogen atmosphere, an ammonia atmosphere, a sulfur dioxide atmosphere, a hydrogen sulfide atmosphere, or a combination atmosphere of any two of these five gases.

8. The preparation method according to claim 1, characterized in that: The sintering includes one-stage sintering and two-stage sintering; the temperature of the one-stage sintering is 200-650°C; the time of the one-stage sintering is 0.5-24h; the temperature of the two-stage sintering is 500-1300°C; the time of the two-stage sintering is 1-72h.

9. A layered oxide positive electrode material with a high exposed (010) crystal plane prepared by the method according to any one of claims 1 to 8.

10. Use of the layered oxide positive electrode material with highly exposed (010) crystal planes as claimed in claim 9 in the preparation of lithium-ion batteries.

Citation Information

Patent Citations

  • Preparation method of nickel-cobalt-manganese / aluminum layered cathode material with large (010) crystal face

    CN112086616A

  • Ternary positive electrode material and preparation method thereof

    CN115626668A