Masonry mortar for reducing saltpetering of plain brick wall and preparation method of masonry mortar

By using low-alkali cement, fly ash and high-reactive silicon fume, combined with polycarboxylic acid water reducer and silicone waterproofing agent, a protective film is formed, which solves the problem of alkalizing in clean water brick walls and improves the compactness of the mortar and alkali resistance reduce the probability of alkali panning and improve the overall appearance and maintenance cost of the building.

CN119019142AInactive Publication Date: 2024-11-26SHANGHAI CONSTRUCTION FOURTH CONSTRUCTION GROUP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411517294.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Clean water brick walls are prone to alkaline, which affects the appearance and maintenance costs of the building. Ordinary silicate cement in existing mortars leads to the migration of water-soluble components and leads to salt deposition.

Method used

Low-alkali cement, fly ash and high-reactive silicon fume, combined with polycarboxylic acid water reducer and silicone waterproofing agent, form a protective film, inhibit water migration and alkali ion transport, and repair micro-micro through water-soluble fluorate. Cracks, reducing alkalinity and moisture migration.

Benefits of technology

It effectively reduces the probability of alkalizing in clean water brick walls, improves the compactness and ion corrosion resistance of the mortar, extends the service life of the mortar, and improves the overall appearance and maintenance cost of the building.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to masonry mortar for reducing efflorescence of a bare brick wall and a preparation method of the masonry mortar. The masonry mortar comprises the following components in percentage by weight: 15%-25% of cement, 2%-5% of fly ash, 1%-2% of silica fume, 60%-80% of sand, 0.01%-0.1% of a water reducing agent, 0.1%-0.4% of redispersible rubber powder, 0.1%-0.4% of water-soluble fluoride and 0.01%-0.1% of a waterproof agent. By adding the redispersible rubber powder and the siloxane waterproof agent, a protective film can be formed inside and outside the mortar, the migration of water in the masonry mortar is reduced, and alkali ions are prevented from being enriched on the surface of a brick wall along with the migration of the water. In the masonry mortar formula disclosed by the invention, all the components have a synergistic effect, so that the saltpetering probability of the plain brick wall is reduced from multiple aspects, and the problem that saltpetering is easily caused during masonry of the traditional plain brick wall can be effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to a masonry mortar for reducing efflorescence of plain brick walls and a preparation method thereof. Background Art

[0002] The exposed brick wall is a typical style of the exterior wall of Chinese historical buildings, with significant artistic and cultural value. Conventional exposed brick walls are mostly built with ordinary mortar, and ordinary Portland cement is often used as a binder in the building materials, which can easily lead to efflorescence on the wall surface, which not only increases the cost of later maintenance, but also affects the appearance of the wall surface. The efflorescence of brick walls is the accumulation of salts formed by the migration of water-soluble components in ordinary Portland cement to the surface with water and precipitation.

[0003] Therefore, how to provide a masonry mortar and a preparation method thereof for reducing efflorescence of exposed brick walls is a technical problem that needs to be urgently solved by those skilled in the art. Summary of the invention

[0004] In order to optimize the finishing effect of exposed brick walls and improve the overall appearance of historical buildings, the present invention provides a masonry mortar for reducing alkali efflorescence of exposed brick walls and a preparation method thereof. The masonry mortar has a low alkali content and can solidify alkali ions and inhibit moisture migration, thereby reducing the probability of alkali efflorescence of exposed brick walls.

[0005] In order to solve the above technical problems, the present invention includes the following technical solutions: A masonry mortar for reducing efflorescence of exposed brick walls, comprising cement, fly ash, silica fume, sand, a water reducing agent, a redispersible rubber powder and a waterproofing agent, wherein the weight percentages of the components of the masonry mortar are: Cement 15%~25%, fly ash 2%~5%, silica fume 1%~2%, sand 60%~80%, water reducer 0.01%~0.1%, redispersible rubber powder 0.1%~0.4%, water-soluble fluoride 0.1%~0.4%, waterproofing agent 0.01%~0.1%.

[0006] Furthermore, 150 g of water is added per kilogram of the masonry mortar when it is used.

[0007] Furthermore, the cement is selected from ordinary Portland cement with an alkali content of less than or equal to 0.6%. Portland cement with low sodium oxide and potassium oxide content can reduce the number of powerful alkali ions and reduce the alkali efflorescence of the plain brick wall caused by masonry mortar.

[0008] Furthermore, the fly ash is selected to be F-type fly ash with low free calcium oxide content and high reaction activity. F-type fly ash can undergo secondary hydration, consume calcium hydroxide produced by cement hydration, and is beneficial to reducing the alkalinity of masonry mortar.

[0009] Furthermore, the silica fume is selected to have a silica content greater than or equal to 90%. Silica fume with a higher silica content has a higher reaction activity, can effectively consume calcium hydroxide produced by cement hydration, and is beneficial to reducing the alkalinity of masonry mortar.

[0010] Furthermore, the sand is selected from machine-made sand or yellow sand, and the sand gradation needs to be continuous. This can improve the compactness of the masonry mortar, thereby helping to inhibit the migration of water inside the masonry mortar and thus reduce the probability of efflorescence of the plain brick wall caused by the masonry mortar.

[0011] Furthermore, the water reducer is a polycarboxylate water reducer with a water reduction efficiency of 20% to 35%. The water reducer can improve the compactness of the masonry mortar, thereby helping to inhibit the migration of water inside the masonry mortar and thus reduce the probability of efflorescence of the plain brick wall caused by the masonry mortar.

[0012] Furthermore, the redispersible rubber powder is selected from ethylene-vinyl acetate copolymer, which can adjust the viscosity of the masonry mortar, thereby providing better workability.

[0013] Furthermore, the waterproofing agent is a siloxane waterproofing agent, wherein the mass ratio of siloxane is ≥ 50%. The waterproofing agent is an organic silicon hydrophobic agent, which is a high molecular weight, three-dimensional mesh waterproofing agent that can be chemically bonded to the surface of a mineral substrate to form a stable, ageing-resistant three-dimensional silicone resin mesh structure, inhibiting the migration of moisture, thereby reducing the probability of internal alkali ions being transmitted to the surface and reducing the possibility of efflorescence in masonry mortar.

[0014] The present invention also provides a method for preparing masonry mortar for reducing efflorescence of plain brick walls, the method comprising the following steps: Step S1, add cement, sand and fly ash into a mixer, and stir slowly for 15-30 seconds until uniform; Step S2, mixing silica fume, redispersible rubber powder and water-soluble fluoride evenly, putting into a blender, and rapidly stirring for 5 to 10 seconds until uniform; Step S3, adding a water reducing agent and a waterproofing agent into a mixer, stirring slowly for 60 to 180 seconds until the mixture is uniform, and obtaining a dry mix of masonry mortar for reducing efflorescence of plain brick walls.

[0015] Compared with the prior art, the present invention has the following advantages and beneficial effects: The present invention provides a masonry mortar for reducing alkali efflorescence of plain brick walls. Low-alkali cement is used, and part of the cement is replaced by mineral admixtures, so that the alkalinity of the masonry mortar can be reduced. By adding redispersible rubber powder and silicone waterproofing agents, a protective film can be formed inside and outside the masonry mortar to reduce the migration of water inside the mortar. By adding water-soluble fluorides, microcracks inside the mortar can be repaired, and the migration of water inside the mortar can be further reduced, thereby avoiding the enrichment of alkali ions on the surface of the brick wall as the water migrates. By adding a water-reducing agent, the strength and density of the masonry mortar can be improved, and its ability to resist ion erosion can be improved. In the masonry mortar formula of the present invention, the synergistic effect between the various components reduces the probability of alkali efflorescence of plain brick walls from multiple aspects, and can effectively solve the problem of easy alkali efflorescence in traditional plain brick wall masonry. DETAILED DESCRIPTION

[0016] The following is a further detailed description of a masonry mortar for reducing efflorescence of exposed brick walls and a preparation method thereof provided by the present invention in conjunction with specific embodiments. The advantages and features of the present invention will become more apparent from the following description.

[0017] A masonry mortar for reducing efflorescence of exposed brick walls, comprising cement, fly ash, silica fume, sand, a water reducing agent, a redispersible rubber powder, a water-soluble fluoride and a waterproofing agent, wherein the weight percentages of the components of the masonry mortar are: Cement 15%~25%, fly ash 2%~5%, silica fume 1%~2%, sand 60%~80%, water reducer 0.01%~0.1%, redispersible rubber powder 0.1%~0.4%, water-soluble fluoride 0.1%~0.4%, waterproofing agent 0.01%~0.1%.

[0018] In particular, 150g of water is added per kilogram of masonry mortar when used.

[0019] In particular, the cement selected is ordinary Portland cement with an alkali content of less than or equal to 0.6%. Portland cement with low sodium oxide and potassium oxide content can reduce the number of powerful alkali ions and reduce the alkali efflorescence of the plain brick wall caused by masonry mortar.

[0020] In particular, the fly ash selected is Class F fly ash with low free calcium oxide content and high reaction activity. Class F fly ash can undergo secondary hydration, consume calcium hydroxide produced by cement hydration, and is beneficial to reducing the alkalinity of masonry mortar.

[0021] In particular, the silica fume is selected to have a silica content greater than or equal to 90%. Silica fume with a higher silica content has a higher reaction activity, can effectively consume the calcium hydroxide produced by cement hydration, and is beneficial to reducing the alkalinity of masonry mortar.

[0022] In particular, the sand should be machine-made sand or yellow sand, and the sand gradation should be continuous. This can improve the compactness of the masonry mortar, which is conducive to inhibiting the migration of water inside the masonry mortar and thus reducing the probability of alkali efflorescence of the plain brick wall caused by the masonry mortar.

[0023] In particular, the water reducer is a polycarboxylate water reducer with a water reduction efficiency of 20% to 35%. Selecting this water reducer can improve the compactness of the masonry mortar, thereby helping to inhibit the migration of water inside the masonry mortar and thus reduce the probability of efflorescence of the plain brick wall caused by the masonry mortar.

[0024] In particular, the redispersible rubber powder is selected from ethylene-vinyl acetate copolymer, which can adjust the viscosity of the masonry mortar, thereby providing better workability.

[0025] In particular, water-soluble fluorides include materials such as magnesium fluorosilicate and zinc fluorosilicate. Such compounds are easily soluble in water and can react with cement hydration products to form water-insoluble precipitates, which are enriched in microcracks to inhibit the transmission of water, thereby improving the efflorescence resistance of low-alkali mortar.

[0026] In particular, the waterproofing agent is a siloxane waterproofing agent, wherein the mass ratio of siloxane is ≥ 50%. The waterproofing agent is an organic silicone hydrophobic agent, a high molecular weight, three-dimensional mesh waterproofing agent, which can be chemically bonded to the surface of the mineral substrate to form a stable, aging-resistant three-dimensional silicone resin mesh structure, inhibiting the migration of moisture, thereby reducing the probability of internal alkali ions being transmitted to the surface and reducing the possibility of efflorescence of masonry mortar.

[0027] The present invention also provides a method for preparing masonry mortar for reducing efflorescence of plain brick walls, the method comprising the following steps: Step S1, add cement, sand and fly ash into a mixer, and stir slowly for 15-30 seconds until uniform; Step S2, mix the silica fume and the redispersible rubber powder evenly, put them into a mixer, and stir them quickly for 5 to 10 seconds until they are uniform; Step S3, adding a water reducing agent and a waterproofing agent into a mixer, stirring slowly for 60 to 180 seconds until the mixture is uniform, and obtaining a dry mix of masonry mortar for reducing efflorescence of plain brick walls.

[0028] Embodiment: According to the formula in Table 1, each component is weighed respectively, and each component is stirred and mixed evenly to obtain the masonry mortar for reducing efflorescence of plain brick walls of the present invention.

[0029] Among them, a common commercially available masonry mortar was selected as the control group.

[0030] Table 2 shows the test results of the performance indicators of masonry mortar used to reduce efflorescence of exposed brick walls.

[0031]

[0032]

[0033] It was observed that the efflorescence area of ​​the exposed brick wall built by the control group exceeded 70%, and no obvious efflorescence occurred in the exposed brick walls built by the mortar of the three groups of embodiments within three months. It can be seen that the masonry mortar for reducing efflorescence of exposed brick walls provided by the present invention adopts low-alkali cement and replaces part of the cement with mineral admixtures, which can reduce the alkalinity of the masonry mortar. By adding redispersible rubber powder and silicone waterproofing agents, a protective film can be formed inside and outside the mortar, reducing the migration of water inside the mortar and avoiding the enrichment of alkali ions on the surface of the brick wall with the migration of water. By adding a water reducer, the strength and density of the mortar can be improved, and its ability to resist ion erosion can be improved. In the masonry mortar formula of the present invention, the synergistic effect between the various components reduces the probability of efflorescence of exposed brick walls from multiple aspects, and can effectively solve the problem of easy efflorescence of traditional exposed brick walls.

[0034] The above examples are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. The above embodiments only express several embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A masonry mortar for reducing efflorescence of exposed brick walls, It is characterized in that The masonry mortar comprises cement, fly ash, silica fume, sand, water reducing agent, redispersible rubber powder, water-soluble fluoride and waterproofing agent. The weight percentage of each component of the masonry mortar is: Cement 15%~25%, fly ash 2%~5%, silica fume 1%~2%, sand 60%~80%, water reducer 0.01%~0.1%, redispersible rubber powder 0.1%~0.4%, water-soluble fluoride 0.1%~0.4%, waterproofing agent 0.01%~0.1%.

2. The masonry mortar for reducing alkali efflorescence of exposed brick walls according to claim 1, It is characterized in that When the masonry mortar is used, 150 g of water is added per kilogram.

3. The masonry mortar for reducing alkali efflorescence of exposed brick walls according to claim 1, It is characterized in that The cement is selected as ordinary Portland cement with an alkali content less than or equal to 0.6%.

4. The masonry mortar for reducing efflorescence of exposed brick walls according to claim 1, It is characterized in that The fly ash is selected from F-type fly ash with low free calcium oxide content and high reaction activity.

5. The masonry mortar for reducing alkali efflorescence of exposed brick walls according to claim 1, It is characterized in that The silica fume is selected to have a silicon dioxide content greater than or equal to 90%.

6. The masonry mortar for reducing alkali efflorescence of exposed brick walls according to claim 1, It is characterized in that The sand can be machine-made sand or yellow sand, and the sand gradation needs to be continuous.

7. The masonry mortar for reducing alkali efflorescence of exposed brick walls according to claim 1, It is characterized in that The water reducing agent is a polycarboxylic acid water reducing agent, and the water reducing efficiency is 20% to 35%.

8. The masonry mortar for reducing efflorescence of exposed brick walls according to claim 1, It is characterized in that The redispersible rubber powder is selected from ethylene-vinyl acetate copolymer.

9. The masonry mortar for reducing alkali efflorescence of exposed brick walls according to claim 1, It is characterized in that The waterproofing agent is a siloxane waterproofing agent, wherein the mass ratio of siloxane is ≥ 50%.

10. The method for preparing the masonry mortar for reducing efflorescence of plain brick walls according to any one of claims 1 to 9, It is characterized in that The method comprises the following steps: Step S1, add cement, sand and fly ash into a mixer, and stir slowly for 15-30 seconds until uniform; Step S2, mixing silica fume, redispersible rubber powder and water-soluble fluoride evenly, putting into a blender, and rapidly stirring for 5 to 10 seconds until uniform; Step S3, adding a water reducing agent and a waterproofing agent into a mixer, stirring slowly for 60 to 180 seconds until the mixture is uniform, and obtaining a dry mix of masonry mortar for reducing alkali efflorescence of plain brick walls.

Citation Information

Patent Citations

  • Economic anti-saltpetering inside and outside walls facing mortar

    CN101628799A

  • Masonry mortar and method for preventing and treating saltpetering of plain brick wall

    CN113480243A

  • Thermal insulation wall protective layer dry material, mortar and wall

    CN113603430A

  • Low-carbon saltpetering-resistant cement-based decorative mortar based on low cement dosage and preparation method thereof