Preparation method of boron carbide ceramic and application of boron carbide ceramic in bulletproof helmet

By detecting the density of boron carbide ceramic body and adjusting the pressing parameters, the problem of insufficient density of traditional preparation methods is solved, and the density and performance of boron carbide ceramics are improved. It is suitable for high-performance bulletproof helmets.

CN119019172AInactive Publication Date: 2024-11-26WUHAN JINXIN NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410962406.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The traditional boron carbide ceramic preparation method has poor density, which limits its wide application in bulletproof equipment.

Method used

By detecting the density of the blank and adjusting the operating parameters of the press according to the helium content value, including pressurization pressure, holding time and pressing speed, the compactness of boron carbide ceramics is improved.

Benefits of technology

It improves the density and comprehensive performance of boron carbide ceramics and enhances its application potential in bulletproof helmets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019172A_ABST
    Figure CN119019172A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation and application of advanced ceramic materials, in particular to a preparation method of boron carbide ceramic and application of the boron carbide ceramic in bulletproof helmets, and relates to a method for preparing a high-performance boron carbide ceramic material and application of the high-performance boron carbide ceramic material in bulletproof helmets. After a green body is pressed, whether the compactness of the green body meets the standard or not is determined according to the comparison result of the helium content detected by a helium leak detector and a preset helium comparison value, and if not, the pressure maintaining time and the pressing speed of a pressing machine during green body pressing are adjusted according to the helium content value. Or the pressurization pressure of the pressing machine during blank pressing is adjusted, and the operation parameters of the pressing machine during blank pressing are controlled, so that the boron carbide ceramic with the characteristics of high hardness, high strength and light weight can be produced, and the protection performance of the bulletproof helmet is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation and application of advanced ceramic materials, and in particular to a preparation method of boron carbide ceramics and application of the same in bulletproof helmets. Background Art

[0002] With the increasing requirements for personal protective equipment in modern warfare, the performance of bulletproof helmets has become a hot topic of research. Boron carbide ceramics are widely used in bulletproof helmets due to their excellent mechanical properties. However, the traditional preparation method of boron carbide ceramics has problems such as high cost and complex process, which limits its wide application in bulletproof equipment.

[0003] Chinese Patent Publication No.: CN112125680A discloses a method for purifying boron carbide micropowder, boron carbide ceramics and a method for preparing boron carbide ceramics. The method for purifying boron carbide micropowder is based on the commercially available W3.5 series boron carbide micropowder raw material for homogenization grinding, vacuum heat treatment purification, and secondary grinding, and the boron carbide slurry is dried and powdered by spray granulation. Boron carbide ceramics are composed of the following components: boron carbide micropowder, liquid carbon black, submicron aluminum nitride micropowder, titanate coupling agent, water-soluble phenolic resin, water-soluble acrylic glue, polyethylene glycol, glycerol, deionized water, whisker-type multi-walled carbon nanotubes, Ti--SiC ternary MAX phase micropowder. The method for preparing boron carbide ceramics is to weigh the components and then perform high-speed ball milling slurrying, spray granulation, green body pressing, and pressureless sintering. It solves the problem of low purity of boron carbide micropowder in the prior art, and at the same time realizes the pressureless sintering preparation of boron carbide ceramics.

[0004] However, the boron carbide ceramics prepared by the traditional boron carbide ceramic preparation method have poor density, which limits its wide application in bulletproof equipment. Summary of the invention

[0005] To this end, the present invention provides a method for preparing a boron carbide ceramic and application of the boron carbide ceramic in a bulletproof helmet, so as to overcome the problem of poor density of the boron carbide ceramic prepared in the prior art.

[0006] To achieve the above object, the present invention provides a method for preparing boron carbide ceramics, comprising:

[0007] Mixing raw materials according to a preset ratio and ball-milling the mixed raw materials, wherein the raw materials at least include boron powder and carbon powder;

[0008] Using a pressing machine to press the processed raw materials into a green body;

[0009] When pressing the green body, a pressure determination parameter is calculated based on the volume and thickness of the green body to determine the pressing pressure of the press when pressing the green body;

[0010] Detecting the compactness of the green body, and determining whether the compactness of the green body meets the standard according to the comparison result of the helium content detected by the helium leak detector and the preset helium comparison value, and if not, adjusting the holding time of the pressing machine when pressing the green body according to the helium content value, or adjusting the pressurization pressure of the pressing machine when pressing the green body;

[0011] If the adjusted holding time exceeds the holding time threshold, the pressing speed of the pressing machine when pressing the green body is adjusted according to the adjusted holding time;

[0012] Sintering the green body that meets the standard density at high temperature;

[0013] The sintered boron carbide ceramic is surface treated to obtain a finished boron carbide ceramic product.

[0014] Furthermore, the method for calculating the pressure determination parameter based on the volume and thickness of the blank is to set:

[0015]

[0016] Wherein, X is the pressure determination parameter, V is the volume of the blank, V0 is the standard volume value, H is the thickness of the blank, and H0 is the standard thickness value.

[0017] Furthermore, the process of determining the pressing pressure of the pressing machine when pressing the green body according to the pressure determination parameter includes:

[0018] Comparing the pressure determination parameter with a preset pressure comparison parameter;

[0019] The pressing pressure of the pressing machine when pressing the green body is determined based on the comparison results.

[0020] Furthermore, a helium test method is used to detect the compactness of the green body. If the compactness of the green body does not meet the standard, the operating parameters of the pressing machine during the green body pressing process are adjusted according to the compactness of the green body.

[0021] Furthermore, when detecting the compactness of the blank, the helium content value detected by the helium leak detector is recorded, and whether the compactness of the blank meets the standard is determined according to the helium content value;

[0022] If the helium content value is less than a preset first helium comparison value, it is determined that the compactness of the blank meets the standard;

[0023] If the helium content value is greater than or equal to the first helium comparison value and less than a preset second helium comparison value, it is determined that the compactness of the green body does not meet the standard, and the holding time of the pressing machine when pressing the green body is adjusted according to the helium content value;

[0024] If the helium content value is greater than or equal to the second helium comparison value, it is determined that the compactness of the green body does not meet the standard, and the pressing pressure of the pressing machine when pressing the green body is adjusted according to the helium content value.

[0025] Furthermore, the method for adjusting the holding time of the pressing machine includes:

[0026] Calculate the holding time adjustment parameters;

[0027] adjusting the holding time of the pressing machine to a corresponding value based on the holding time adjustment parameter;

[0028] The pressure holding time adjustment parameter is the difference between the helium content value and the first helium comparison value.

[0029] Furthermore, the adjusted holding time is compared with a preset holding time threshold. If the adjusted holding time is greater than the holding time threshold, the holding time is set to the holding time threshold, and the pressing speed of the pressing machine when pressing the blank is adjusted according to the adjusted holding time.

[0030] Furthermore, the method for adjusting the pressing speed of the pressing machine includes:

[0031] Calculate the pressing speed adjustment parameter;

[0032] adjusting the pressing speed of the pressing machine to a corresponding value based on the pressing speed adjustment parameter;

[0033] The pressing speed adjustment parameter is the difference between the adjusted holding time and the holding time threshold.

[0034] Furthermore, the method for adjusting the pressurization pressure of the press machine includes:

[0035] Calculate the pressure adjustment parameter of the pressurization;

[0036] adjusting the pressurizing pressure of the press machine to a corresponding value based on the pressurizing pressure adjustment parameter;

[0037] The pressurization pressure adjustment parameter is the difference between the helium content value and the second helium comparison value.

[0038] The invention also provides a bulletproof helmet, comprising a boron carbide ceramic layer prepared by the preparation method of the boron carbide ceramic.

[0039] Compared with the prior art, the present invention has the beneficial effect that the present invention improves the density of boron carbide ceramics by detecting the density of the green body and adjusting the operating parameters of the pressing machine when pressing the green body according to the detection results, while improving the comprehensive performance of the boron carbide ceramics.

[0040] Furthermore, the present invention determines parameters by calculating pressure. When the green body is pressed, the pressing pressure set by the pressing machine is closely related to the volume and thickness of the green body. The pressure determination parameter calculated by the volume and thickness of the green body is a representative parameter of the pressing pressure set by the pressing machine. By determining the pressing pressure during green body pressing according to the pressure determination parameter, the accuracy of the set pressing pressure can be improved, thereby improving the density of the boron carbide ceramic.

[0041] Furthermore, the present invention can improve the accuracy of the set pressure by setting a first pressure comparison parameter and a second pressure comparison parameter, and determine the pressure applied by the pressing machine when pressing the green body based on the comparison result of the pressure determination parameter with the first pressure comparison parameter and the second pressure comparison parameter, thereby further improving the density of the boron carbide ceramic.

[0042] Furthermore, in actual production, the density of the green body increases with the increase of pressure. During the pressing process, the pressure has a great influence on the density, strength and porosity of the green body. If the pressure is too small, the green body cannot reach the maximum densification, which affects the sintering densification process. If the pressure is too large, defects similar to layer cracking will appear. Only when the pressure is moderate can an ideal green body be pressed out. Therefore, in the present invention, when the helium content value is greater than or equal to the second helium comparison value, the helium content value at this time is relatively large, and the pressure of the pressing machine is adjusted when pressing the green body, thereby increasing the density of the green body and further improving the density of the boron carbide ceramic.

[0043] Furthermore, since the appropriate holding time can effectively remove the gas retained in the green body when pressing the green body, when the helium content value is greater than or equal to the first helium comparison value and less than the second helium comparison value, the helium content value at this time is relatively small. By adjusting the holding time of the pressing machine when pressing the green body, the density of the boron carbide ceramic is further improved.

[0044] Furthermore, the present invention can improve the accuracy of the set holding time by setting a first preset holding time comparison parameter and a second preset holding time comparison parameter, and adjusting the holding time of the pressing machine when pressing the green body according to the comparison result of the holding time adjustment parameter and the preset holding time comparison parameter, thereby further improving the density of the boron carbide ceramic.

[0045] Furthermore, the present invention can improve the accuracy of the set pressing speed by setting a first preset pressing speed comparison parameter and a second preset pressing speed comparison parameter, and adjusting the pressing speed of the pressing machine when pressing the green body according to the comparison result of the pressing speed adjustment parameter and the preset pressing speed comparison parameter, thereby further improving the density of the boron carbide ceramic.

[0046] Furthermore, the present invention further improves the accuracy of the set pressurization pressure by adjusting the pressurization pressure, thereby further improving the density of the boron carbide ceramic. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is a flow chart of a method for preparing boron carbide ceramics according to an embodiment of the present invention;

[0048] Figure 2 This is a flow chart of step S2 in the method for preparing boron carbide ceramics according to an embodiment of the present invention. DETAILED DESCRIPTION

[0049] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0050] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.

[0051] See also Figure 1 As shown, the preparation method of the boron carbide ceramic of the present invention comprises:

[0052] Step S1, raw material processing;

[0053] Mixing raw materials according to a preset ratio and ball-milling the mixed raw materials, wherein the raw materials at least include boron powder and carbon powder;

[0054] Step S2, pressing the green body;

[0055] Using a pressing machine to press the processed raw materials into a green body;

[0056] Step S2 includes:

[0057] Step S21, when pressing the green body, calculating the pressure determination parameter based on the volume and thickness of the green body to determine the pressing pressure of the pressing machine when pressing the green body;

[0058] Step S22, detecting the compactness of the green body, and determining whether the compactness of the green body meets the standard according to the comparison result of the helium content detected by the helium leak detector and the preset helium comparison value; if not, adjusting the holding time of the pressing machine when pressing the green body according to the helium content value, or adjusting the pressurization pressure of the pressing machine when pressing the green body;

[0059] Step S23, if the adjusted holding time exceeds the holding time threshold, adjusting the pressing speed of the pressing machine when pressing the green body according to the adjusted holding time;

[0060] Step S3, high temperature sintering;

[0061] Sintering the green body that meets the standard density at high temperature;

[0062] Step S4, surface treatment;

[0063] The sintered boron carbide ceramic is surface treated to obtain a finished boron carbide ceramic product.

[0064] The raw materials are ball-milled to increase the activity of the powder.

[0065] In this embodiment, the green body is preferably sintered under the protection of an inert gas to promote the formation of boron carbide.

[0066] The sintered boron carbide ceramics are surface treated to improve their surface finish and overall strength.

[0067] The raw material ratio is a mass ratio of boron powder to carbon powder of 4:1, wherein the boron powder and the carbon powder are selected from high-purity boron powder and high-purity carbon powder, preferably the purity of the high-purity boron powder is greater than or equal to 99.9%, and preferably the purity of the high-purity carbon powder is greater than or equal to 99.9%.

[0068] Other ingredients may be added to the raw materials to adjust the properties of the materials, including adding sintering aids or performing surface modification to improve the compactness during the sintering process and the properties of the final product, which is not specifically limited in this embodiment.

[0069] When the raw material is ball-milled, it can be mixed with a binder (such as flax glue, phenolic resin, sodium alginate, etc.) and an additive (such as zinc oxide, light calcium powder), and deionized water is added for ball-milling. After the ball-milling is completed, the slurry can achieve the desired stability and fluidity by controlling the cooling rate and the standing time. The above is just an example.

[0070] When high-temperature sintering is performed, the preferred sintering temperature is 2000-2200° C. and the sintering time is 2-4 hours.

[0071] The sintering method can be hot pressing sintering or plasma sintering.

[0072] The surface treatment of the sintered boron carbide ceramics includes machining, polishing, coating and other processing steps.

[0073] Specifically, the method for calculating the pressure determination parameters based on the volume and thickness of the blank is to set:

[0074]

[0075] Wherein, X is the pressure determination parameter, V is the volume of the blank, V0 is the standard volume value, H is the thickness of the blank, and H0 is the standard thickness value.

[0076] In this embodiment, the method for setting the standard volume value V0 and the standard thickness value H0 is to select at least 500 volume values ​​and thickness values ​​of boron carbide ceramics used to prepare helmets, and calculate the average value of the volume values ​​and the average value of the thickness values ​​of the at least 500 boron carbide ceramics used to prepare helmets, and use the calculated average value of the volume value as the standard volume value, and use the calculated average value of the thickness value as the standard thickness value.

[0077] The present invention determines parameters by calculating pressure. When a green body is pressed, the pressing pressure set by the press is closely related to the volume and thickness of the green body. The pressure determination parameter calculated by the volume and thickness of the green body is a representative parameter of the pressing pressure set by the press. The pressing pressure during green body pressing is determined according to the pressure determination parameter, which can improve the accuracy of the set pressing pressure, thereby improving the density of the boron carbide ceramic.

[0078] Specifically, the process of determining the pressing pressure of the pressing machine when pressing the green body according to the pressure determination parameter includes:

[0079] Comparing the pressure determination parameter with a preset pressure comparison parameter;

[0080] The pressing pressure of the pressing machine when pressing the green body is determined based on the comparison results.

[0081] Specifically, the preset pressure comparison parameter includes a first pressure comparison parameter X1 and a second pressure comparison parameter X2, the first pressure comparison parameter X1 is less than the second pressure comparison parameter X2, the pressure determination parameter is compared with the first pressure comparison parameter X1 and the second pressure comparison parameter X2 respectively, and the pressurization pressure of the pressing machine when pressing the blank is determined according to the comparison result;

[0082] Wherein, if X<X1, the pressing pressure of the pressing machine when pressing the green body is set to F=F0×(X / X1);

[0083] If X1≤X<X2, the pressing pressure of the pressing machine when pressing the green body is set to F=F0×[2X / (X1+X2)];

[0084] If X2≤X, the pressing pressure of the pressing machine when pressing the green body is set to F=F0×(X / X2).

[0085] Specifically, when determining the first pressure comparison parameter and the second pressure comparison parameter of the present embodiment, at least 1000 volumes and thicknesses of the blanks whose densities meet the standards are selected, and the corresponding at least 1000 pressure determination parameters are calculated to construct a pressure determination parameter data set. The pressure determination parameter is used as a random variable, and the random variable obeys a probability density function. Then, a normal distribution curve can be constructed according to the probability density function, and the 95% confidence interval of the normal distribution curve is determined. The pressure determination parameter corresponding to the midpoint of the 95% confidence interval is determined as the first pressure comparison parameter, and the pressure determination parameter corresponding to the lower limit of the 95% confidence interval is determined as the second pressure comparison parameter. Constructing a probability density function and constructing a normal distribution curve based on the probability density function are commonly used technical means in statistics, which will not be repeated here.

[0086] The present invention sets a first pressure comparison parameter and a second pressure comparison parameter, and determines the pressing pressure of the pressing machine when pressing the green body according to the comparison result of the pressure determination parameter with the first pressure comparison parameter and the second pressure comparison parameter, so as to improve the accuracy of the set pressing pressure and further improve the density of the boron carbide ceramic.

[0087] Specifically, a helium test method is used to detect the compactness of the green body. If the compactness of the green body does not meet the standard, the operating parameters of the pressing machine during the green body pressing process are adjusted according to the compactness of the green body.

[0088] The specific operation of the helium test method is to fill the test medium with helium. If there are loose places, the helium can be detected on the surface of the inspected part using a helium leak detector. The current helium leak detector can detect the presence of one ten-millionth of helium in the gas, which is equivalent to a helium leakage rate of 1cm^3 / a under standard conditions. Therefore, it has a high sensitivity.

[0089] Specifically, when testing the compactness of the blank, the helium content value detected by the helium leak detector is recorded, and whether the compactness of the blank meets the standard is determined according to the helium content value;

[0090] If the helium content value is less than a preset first helium comparison value, it is determined that the compactness of the blank meets the standard;

[0091] If the helium content value is greater than or equal to the first helium comparison value and less than a preset second helium comparison value, it is determined that the compactness of the green body does not meet the standard, and the holding time of the pressing machine when pressing the green body is adjusted according to the helium content value;

[0092] If the helium content value is greater than or equal to the second helium comparison value, it is determined that the compactness of the green body does not meet the standard, and the pressing pressure of the pressing machine when pressing the green body is adjusted according to the helium content value.

[0093] In this embodiment, the first helium contrast value is set to 1.2 cm^3 / a, and the second helium contrast value is set to 1.4 cm^3 / a, which can also be set according to actual conditions.

[0094] In actual production, the density of the green body increases with the increase of pressure. During the pressing process, the pressure has a great influence on the density, strength and porosity of the green body. If the pressure is too small, the green body cannot reach the maximum densification, which affects the sintering densification process. If the pressure is too large, defects similar to layer cracking will appear. Only when the pressure is moderate can an ideal green body be pressed out. Therefore, in the present invention, when the helium content value is greater than or equal to the second helium comparison value, the helium content value at this time is relatively large, and the pressure of the pressing machine is adjusted when pressing the green body, thereby increasing the density of the green body and further improving the density of the boron carbide ceramic.

[0095] Since a suitable holding time can effectively remove the gas retained in the green body when pressing the green body, when the helium content value is greater than or equal to the first helium comparison value and less than the second helium comparison value, the helium content value at this time is relatively small. By adjusting the holding time of the pressing machine when pressing the green body, the density of the boron carbide ceramic is further improved.

[0096] Specifically, the method for adjusting the holding time of the pressing machine includes:

[0097] Calculate the holding time adjustment parameters;

[0098] adjusting the holding time of the pressing machine to a corresponding value based on the holding time adjustment parameter;

[0099] The pressure holding time adjustment parameter is the difference between the helium content value and the first helium comparison value.

[0100] Specifically, the holding time adjustment parameter is compared with the preset holding time comparison parameter to adjust the holding time to a corresponding value, the preset holding time comparison parameter includes a first preset holding time comparison parameter and a second preset holding time comparison parameter, the first preset holding time comparison parameter is smaller than the second preset holding time comparison parameter, wherein,

[0101] When the holding time adjustment parameter is less than or equal to the first preset holding time comparison parameter, selecting the first holding time adjustment coefficient 1.2 to adjust the holding time to the corresponding value;

[0102] When the holding time adjustment parameter is greater than the first preset holding time comparison parameter and less than or equal to the second preset holding time comparison parameter, the second holding time adjustment coefficient 1.3 is selected to adjust the holding time to the corresponding value;

[0103] When the holding time adjustment parameter is greater than the second preset holding time comparison parameter, selecting the third holding time adjustment coefficient 1.4 to adjust the holding time to a corresponding value;

[0104] The adjusted holding time is the product of the initial holding time setting value and the holding time adjustment coefficient.

[0105] It can be understood that the initial holding time setting value corresponds to the pressurization pressure determined according to the pressure determination parameter.

[0106] In this embodiment, when setting the first preset holding time comparison parameter and the second preset holding time comparison parameter, a probability function can be used for determination. Specifically, at least 1000 times of density experimental data are selected, and the corresponding at least 1000 times of holding time adjustment parameters are calculated to construct a holding time adjustment parameter data set. The holding time adjustment parameter is used as a random variable, and the random variable obeys the probability density function. Then, a normal distribution curve can be constructed according to the probability density function, and the 95% confidence interval of the normal distribution curve is determined. The holding time adjustment parameter corresponding to the midpoint of the 95% confidence interval is determined as the first preset holding time comparison parameter, and the holding time adjustment parameter corresponding to the lower limit of the 95% confidence interval is determined as the second preset holding time comparison parameter.

[0107] The present invention can improve the accuracy of the set holding time by setting a first preset holding time comparison parameter and a second preset holding time comparison parameter, and adjust the holding time of the pressing machine when pressing the green body according to the comparison result of the holding time adjustment parameter and the preset holding time comparison parameter, thereby further improving the density of the boron carbide ceramic.

[0108] Specifically, the adjusted holding time is compared with the preset holding time threshold. If the adjusted holding time is greater than the holding time threshold, the holding time is set to the holding time threshold, and the pressing speed of the pressing machine when pressing the blank is adjusted according to the adjusted holding time.

[0109] In this embodiment, the pressure holding time threshold is 1.1×T0, where T0 is the initial pressure holding time setting value.

[0110] Specifically, the method for adjusting the pressing speed of the pressing machine includes:

[0111] Calculate the pressing speed adjustment parameter;

[0112] adjusting the pressing speed of the pressing machine to a corresponding value based on the pressing speed adjustment parameter;

[0113] The pressing speed adjustment parameter is the difference between the adjusted holding time and the holding time threshold.

[0114] Specifically, the pressing speed adjustment parameter is compared with a preset pressing speed comparison parameter to adjust the pressing speed to a corresponding value, the preset pressing speed comparison parameter includes a first preset pressing speed comparison parameter and a second preset pressing speed comparison parameter, the first preset pressing speed comparison parameter is smaller than the second preset pressing speed comparison parameter, wherein,

[0115] When the pressing speed adjustment parameter is less than or equal to the first preset pressing speed comparison parameter, selecting the first pressing speed adjustment coefficient 0.95 to adjust the pressing speed to the corresponding value;

[0116] When the pressing speed adjustment parameter is greater than the first preset pressing speed comparison parameter and less than or equal to the second preset pressing speed comparison parameter, selecting the second pressing speed adjustment coefficient 0.9 to adjust the pressing speed to the corresponding value;

[0117] When the pressing speed adjustment parameter is greater than the second preset pressing speed comparison parameter, selecting the third pressing speed adjustment coefficient 0.85 to adjust the pressing speed to the corresponding value;

[0118] The adjusted pressing speed is the product of the initial pressing speed setting value and the pressing speed adjustment coefficient.

[0119] It can be understood that the initial pressing speed setting value corresponds to the pressing pressure determined according to the pressure determination parameter.

[0120] In this embodiment, when setting the first preset pressing speed comparison parameter and the second preset pressing speed comparison parameter, a probability function can be used for determination. Specifically, at least 1000 times of density experimental data are selected, and the corresponding pressing speed adjustment parameters of at least 1000 times are calculated to construct a pressing speed adjustment parameter data set. The pressing speed adjustment parameter is used as a random variable, and the random variable obeys the probability density function. Then, a normal distribution curve can be constructed according to the probability density function, and the 95% confidence interval of the normal distribution curve is determined. The pressing speed adjustment parameter corresponding to the midpoint of the 95% confidence interval is determined as the first preset pressing speed comparison parameter, and the pressing speed adjustment parameter corresponding to the lower limit of the 95% confidence interval is determined as the second preset pressing speed comparison parameter.

[0121] The present invention can improve the accuracy of the set pressing speed by setting a first preset pressing speed comparison parameter and a second preset pressing speed comparison parameter, and adjust the pressing speed of the pressing machine when pressing the green body according to the comparison result of the pressing speed adjustment parameter and the preset pressing speed comparison parameter, thereby further improving the density of the boron carbide ceramic.

[0122] Specifically, the method for adjusting the pressurization pressure of the press machine includes:

[0123] Calculate the pressure adjustment parameter of the pressurization;

[0124] adjusting the pressurizing pressure of the press machine to a corresponding value based on the pressurizing pressure adjustment parameter;

[0125] The pressurization pressure adjustment parameter is the difference between the helium content value and the second helium comparison value.

[0126] Specifically, the pressurization pressure adjustment parameter is compared with the preset pressurization pressure comparison parameter to adjust the pressurization pressure to a corresponding value, the preset pressurization pressure comparison parameter includes a first preset pressurization pressure comparison parameter and a second preset pressurization pressure comparison parameter, the first preset pressurization pressure comparison parameter is smaller than the second preset pressurization pressure comparison parameter, wherein,

[0127] When the pressurizing pressure adjustment parameter is less than or equal to the first preset pressurizing pressure comparison parameter, selecting the first pressurizing pressure adjustment coefficient 1.015 to adjust the pressurizing pressure to the corresponding value;

[0128] When the pressurization pressure adjustment parameter is greater than the first preset pressurization pressure comparison parameter and less than or equal to the second preset pressurization pressure comparison parameter, the second pressurization pressure adjustment coefficient 1.020 is selected to adjust the pressurization pressure to the corresponding value;

[0129] When the pressurizing pressure adjustment parameter is greater than the second preset pressurizing pressure comparison parameter, selecting the third pressurizing pressure adjustment coefficient 1.025 to adjust the pressurizing pressure to a corresponding value;

[0130] The adjusted boost pressure is the product of the boost pressure determined according to the pressure determination parameter and the boost pressure adjustment coefficient.

[0131] In this embodiment, when the first preset pressurization pressure comparison parameter is set to be smaller than the second preset pressurization pressure comparison parameter, a probability function can be used for determination. Specifically, at least 1000 times of density experimental data are selected, and the corresponding pressurization pressure adjustment parameters of at least 1000 times are calculated to construct a pressurization pressure adjustment parameter data set. The pressurization pressure adjustment parameter is taken as a random variable, and the random variable obeys the probability density function. Then, a normal distribution curve can be constructed according to the probability density function, and the 95% confidence interval of the normal distribution curve is determined. The pressurization pressure adjustment parameter corresponding to the midpoint of the 95% confidence interval is determined as the first preset pressurization pressure comparison parameter, and the pressurization pressure adjustment parameter corresponding to the lower limit of the 95% confidence interval is determined as the second preset pressurization pressure comparison parameter.

[0132] The present invention further improves the accuracy of the set pressurization pressure by adjusting the pressurization pressure, thereby further improving the density of the boron carbide ceramic.

[0133] This embodiment also provides a bulletproof helmet, including a boron carbide ceramic layer prepared by the preparation method of boron carbide ceramic.

[0134] Boron carbide ceramics are ideal materials for protective equipment such as bulletproof helmets due to their light weight, ultra-high hardness and high elastic modulus. They have the following advantages

[0135] Improve bulletproof performance: The high hardness of boron carbide ceramics enables it to effectively resist the penetration of high-speed impact objects such as bullets, thereby reducing the risk of head injuries.

[0136] Reduce weight: Compared with traditional metal materials, boron carbide ceramics have lower density and lighter weight, which helps to reduce the overall weight of the ballistic helmet and improve the comfort of the wearer.

[0137] Enhanced antioxidant properties: Through special preparation processes and formula adjustments, the antioxidant properties of boron carbide ceramics can be further improved, allowing them to maintain stable performance under high temperatures or harsh environments.

[0138] Improve the ability to resist multiple hits: By optimizing the sintering process and toughening and reinforcement technology, boron carbide ceramic materials with higher toughness can be prepared, thereby improving the ability of bulletproof helmets to resist multiple bullet hits.

[0139] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

[0140] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing boron carbide ceramics, characterized in that: include: Mixing raw materials according to a preset ratio and ball-milling the mixed raw materials, wherein the raw materials at least include boron powder and carbon powder; Using a pressing machine to press the processed raw materials into a green body; When pressing the green body, a pressure determination parameter is calculated based on the volume and thickness of the green body to determine the pressing pressure of the press when pressing the green body; Detecting the compactness of the green body, and determining whether the compactness of the green body meets the standard according to the comparison result of the helium content detected by the helium leak detector and the preset helium comparison value, and if not, adjusting the holding time of the pressing machine when pressing the green body according to the helium content value, or adjusting the pressurization pressure of the pressing machine when pressing the green body; If the adjusted holding time exceeds the holding time threshold, the pressing speed of the pressing machine when pressing the green body is adjusted according to the adjusted holding time; Sintering the green body that meets the standard density at high temperature; The sintered boron carbide ceramic is surface treated to obtain a finished boron carbide ceramic product.

2. The method for preparing boron carbide ceramics according to claim 1, characterized in that: The method for calculating the pressure determination parameters based on the volume and thickness of the blank is to set: Wherein, X is the pressure determination parameter, V is the volume of the blank, V0 is the standard volume value, H is the thickness of the blank, and H0 is the standard thickness value.

3. The method for preparing boron carbide ceramics according to claim 2, characterized in that: The process of determining the pressing pressure of the pressing machine when pressing the green body according to the pressure determination parameter comprises: Comparing the pressure determination parameter with a preset pressure comparison parameter; The pressing pressure of the pressing machine when pressing the green body is determined based on the comparison results.

4. The method for preparing boron carbide ceramics according to claim 3, characterized in that: The compactness of the green body is tested by a helium test method. If the compactness of the green body does not meet the standard, the operating parameters of the pressing machine during the green body pressing process are adjusted according to the compactness of the green body.

5. The method for preparing boron carbide ceramics according to claim 4, characterized in that: When testing the compactness of the blank, the helium content value detected by the helium leak detector is recorded, and whether the compactness of the blank meets the standard is determined according to the helium content value; If the helium content value is less than a preset first helium comparison value, it is determined that the compactness of the blank meets the standard; If the helium content value is greater than or equal to the first helium comparison value and less than a preset second helium comparison value, it is determined that the compactness of the green body does not meet the standard, and the holding time of the pressing machine when pressing the green body is adjusted according to the helium content value; If the helium content value is greater than or equal to the second helium comparison value, it is determined that the compactness of the green body does not meet the standard, and the pressing pressure of the pressing machine when pressing the green body is adjusted according to the helium content value.

6. The method for preparing boron carbide ceramics according to claim 5, characterized in that: The method for adjusting the holding time of the pressing machine includes: Calculate the holding time adjustment parameters; adjusting the holding time of the pressing machine to a corresponding value based on the holding time adjustment parameter; The pressure holding time adjustment parameter is the difference between the helium content value and the first helium comparison value.

7. The method for preparing boron carbide ceramics according to claim 6, characterized in that: The adjusted holding time is compared with the preset holding time threshold. If the adjusted holding time is greater than the holding time threshold, the holding time is set to the holding time threshold, and the pressing speed of the pressing machine when pressing the blank is adjusted according to the adjusted holding time.

8. The method for preparing boron carbide ceramics according to claim 7, characterized in that: The method for adjusting the pressing speed of the pressing machine includes: Calculate the pressing speed adjustment parameter; adjusting the pressing speed of the pressing machine to a corresponding value based on the pressing speed adjustment parameter; The pressing speed adjustment parameter is the difference between the adjusted holding time and the holding time threshold.

9. The method for preparing boron carbide ceramics according to claim 8, characterized in that: The method for adjusting the pressurizing pressure of the pressing machine includes: Calculate the pressure adjustment parameter of the pressurization; adjusting the pressurizing pressure of the press machine to a corresponding value based on the pressurizing pressure adjustment parameter; The pressurization pressure adjustment parameter is the difference between the helium content value and the second helium comparison value.

10. A bulletproof helmet, characterized in that: The invention comprises a boron carbide ceramic layer prepared by the method according to any one of claims 1 to 9.