Modified cellulose based on nucleophilic addition effect, preparation method and application

By performing nucleophilic addition reaction in cellulose to generate modified cellulose, and high-speed mixing and melt extrusion with HDPE, the problem of poor compatibility between HDPE and cellulose is solved, and the mechanical properties of HDPE are significantly improved, thus achieving the realization of Good dispersion and mechanical properties of cellulose in HDPE are improved.

CN119019575APending Publication Date: 2024-11-26HEFEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411136086.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, HDPE and cellulose have poor compatibility, resulting in less obvious improvement in dispersion and mechanical properties of cellulose in HDPE resin, and the process is complicated and not suitable for industrial promotion.

Method used

By introducing nucleophilic addition reactions into cellulose, modified cellulose is generated and mixed and melt extruded with HDPE at high speed to form modified fibers based on nucleophilic addition action to improve the interface compatibility and mechanical properties of cellulose and HDPE.

Benefits of technology

It significantly improves the mechanical properties of HDPE, including the improvement of tensile strength and bending strength, and the modified cellulose has renewable properties and a simple preparation process, suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019575A_ABST
    Figure CN119019575A_ABST
Patent Text Reader

Abstract

The invention discloses modified cellulose based on nucleophilic addition, a preparation method and application, and the preparation method of the modified cellulose comprises the following steps: S1, placing cellulose in dimethyl sulfoxide at normal temperature to prepare a suspension; and S2, under the protection of inert gas, adding a premixed solution of isocyanate ethyl acrylate and dibutyltin laurate into the turbid liquid in the S1 for reaction, and then precipitating, washing and drying to obtain the modified cellulose. According to the preparation method, cellulose and isocyanate ethyl acrylate are subjected to nucleophilic addition reaction, hydroxyl of the cellulose can react with isocyanate groups of the isocyanate ethyl acrylate to generate carbamate bonds, and the hydrophobicity of the cellulose is improved; meanwhile, a carbon-carbon double bond of isocyanate ethyl acrylate can be subjected to free radical type polymerization reaction with HDPE, so that the interfacial compatibility between the filler and resin is improved, and the mechanical property of HDPE is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite materials, and in particular to modified cellulose based on nucleophilic addition, a preparation method and application thereof. Background Art

[0002] At present, reinforced high-density polyethylene (HDPE) has the advantages of high strength and strong stability, so it has a wide range of uses, including corrosion-resistant pipes, geomembranes and plastic wood. In the system of reinforced HDPE and reinforcing agent fillers, different types of fillers are targeted at different functional characteristics. There are many reinforcing fillers, among which inorganic fillers include calcium carbonate, talcum powder, glass fiber, etc., and organic fillers include cellulose, etc. For cellulose, it has the advantages of renewability, high mechanical properties and low cost, and biomass fillers have broad application prospects. There is a problem of low compatibility when adding cellulose to HDPE resin. The compatibility between resin and cellulose can be increased by adding and reacting methods.

[0003] At present, the main methods to improve the mechanical properties by improving the compatibility of HDPE and cellulose are to hydrophobically modify cellulose or to increase the capacity of the PE / cellulose system by adding a compatibilizer. For example, by reacting the amino and imino groups grafted on the cellulose side chains with the epoxy groups of epoxidized PE to form a cellulose-grafted PE compatibilizer, the interfacial compatibility of HDPE and cellulose microcrystals is improved, and the dispersibility of cellulose microcrystals in the PE matrix is ​​improved. Therefore, high-strength and high-modulus cellulose microcrystals have a better reinforcing effect on PE, improving the flexural strength and impact strength of PE materials. In addition, PE-g-MAH is used to increase the compatibility between the fiber and the resin matrix, and the plant fiber is modified with silane to improve the mechanical properties of PE plastics. For example, cellulose is modified by diphenylmethane diisocyanate, which can be used to toughen special materials for HDPE plastic chairs. The above examples have the problem that the cellulose modification process is complicated and the modification effect is not obvious; or there is no stable chemical bond connection between cellulose and the resin matrix, and it only relies on intermolecular forces; or the reaction process between the prepared cellulose and PE compatibilizer is complicated, the material performance is not greatly enhanced, and it is not suitable for industrial promotion. Summary of the invention

[0004] Based on the problems existing in the background technology, the present invention proposes a modified cellulose based on nucleophilic addition, a preparation method and an application, which overcomes the problem of poor compatibility between cellulose and HDPE and significantly improves the mechanical properties of HDPE.

[0005] The present invention provides a method for preparing modified cellulose based on nucleophilic addition, and the method steps are as follows:

[0006] S1: Under normal temperature, cellulose is dissolved in dimethyl sulfoxide by stirring to prepare a suspension;

[0007] S2: Under the protection of inert gas, a premixed solution of ethyl isocyanate acrylate and dibutyltin laurate is added to the suspension of S1 to react, and then precipitated, washed and dried to obtain modified cellulose.

[0008] Preferably, the cellulose concentration in S1 is 0.99-2.44 wt %, the stirring speed is 80-100 rpm / min, and the stirring time is 0.5-2 h.

[0009] Preferably, the mass ratio of cellulose, ethyl isocyanate acrylate and dibutyltin laurate is 1:5.68-6.25:0.0057-0.019.

[0010] Preferably, the reaction temperature in S2 is 50-85° C., and the reaction time is 2-3 h.

[0011] The modified cellulose based on nucleophilic addition is prepared by the above method proposed by the present invention.

[0012] The present invention proposes the application of the modified cellulose based on nucleophilic addition in reinforced HDPE.

[0013] Preferably, the method comprises the following steps: mixing HDPE, modified cellulose and di-tert-butyl peroxide at high speed and then melt-extruding them.

[0014] Preferably, the mass ratio of HDPE, modified cellulose and di-tert-butyl peroxide is 1:0.10-0.40:0.0010-0.0040.

[0015] Preferably, the high-speed mixing temperature is 30-45° C. and the time is 1-2 h.

[0016] Preferably, the conditions for melt extrusion are: screw speed of 200-400 rpm, feeding rate of 5-7 Hz, and extrusion temperature zones are set to 170, 170, 175, 180, 180, 175, 170, 165°C.

[0017] Beneficial technical effects of the present invention:

[0018] (1) The present invention utilizes a nucleophilic addition reaction between cellulose and ethyl isocyanate acrylate, whereby the hydroxyl groups in the cellulose can react with the isocyanate groups in the ethyl isocyanate acrylate to form carbamate bonds, thereby increasing the hydrophobicity of the cellulose.

[0019] (2) The isocyanate ethyl acrylate introduced in the present invention has isocyanate and vinyl functional groups, wherein the carbon-carbon double bond of the vinyl group can undergo a free radical polymerization reaction with HDPE. The initiator is decomposed into free radicals by heat, and the free radicals attack the HDPE macromolecular chain to generate HDPE·, which then reacts with the vinyl double bond of the isocyanate ethyl acrylate, further improving the interfacial compatibility between the HDPE resin and the cellulose filler, and at the same time can improve the mechanical properties of HDPE.

[0020] (3) The modified cellulose of the present invention has the characteristics of being renewable, chemically functionalized and having a simple preparation process. The modified cellulose can give full play to the characteristics of the rigid structure of fiber-reinforced plastics in the HDPE matrix. In the composite modified material, the fiber bears a large load stress, and the matrix resin supports the fiber and transmits the external load through the shear stress on the interface with the fiber, thereby improving the mechanical properties of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Infrared spectra of the HDPE, CE, AOI-CE and HDPE / AOI-CE samples proposed in the present invention;

[0022] Figure 2 The water contact angle diagrams of CE and AOI-CE proposed in the present invention;

[0023] Figure 3 Schematic diagram of the synthesis mechanism of AOI-CE proposed in the present invention;

[0024] Figure 4 Schematic diagram of the preparation mechanism of the HDPE / AOI-CE composite material proposed in the present invention. DETAILED DESCRIPTION

[0025] The present invention will be further explained below in conjunction with specific embodiments.

[0026] Example 1

[0027] The application of the modified cellulose based on nucleophilic addition in the enhanced HDPE proposed by the present invention comprises the following steps:

[0028] S1: Under room temperature conditions, 0.5 kg of cellulose (CE) was placed in 25 kg of dimethyl sulfoxide (DMSO) and stirred at 100 rpm / min for 0.5 h to prepare a suspension.

[0029] S2: Under N2 protection, a premixed solution of 2.84 kg of ethyl isocyanate acrylate (AOI) and 4.26 g of dibutyltin laurate (DBTDL) was added to the above suspension, the reaction temperature was 75°C, and the mixing reaction was carried out for 3 hours. After the reaction was completed, 37.5 kg of methanol was added to generate a precipitate, which was then washed and dried to obtain modified cellulose AOI-CE.

[0030] S3: Weigh 0.3 kg of the above AOI-CE, add 1 kg of HDPE and 4 g of di-tert-butyl peroxide (DTBP), and mix at high speed for 1 hour to obtain a masterbatch.

[0031] S4: The masterbatch described in S3 was melt-extruded, the screw speed was 400 rpm, the feeding rate was 5 Hz, and the extrusion temperature zones were set to 170, 170, 175, 180, 180, 175, 170, and 165°C.

[0032] Example 2

[0033] The application of the modified cellulose based on nucleophilic addition in the enhanced HDPE proposed by the present invention comprises the following steps:

[0034] S1: At room temperature, 0.5 kg of CE was placed in 50 kg of DMSO and stirred at 100 rpm / min for 0.5 h to prepare a suspension.

[0035] S2: Under N2 protection, add 2.84 kg of AOI and 4.26 g of DBTDL premixed solution to the above suspension, react at 75°C, and mix for 3 hours. After the reaction is completed, add 75.0 kg of methanol to generate a precipitate, which is then washed and dried to obtain AOI-CE.

[0036] S3: Weigh 0.3 kg of the above AOI-CE, add 1 kg of HDPE and 4 g of DTBP, and mix at high speed for 1 hour to obtain a masterbatch.

[0037] S4: The masterbatch described in S3 was melt-extruded, the screw speed was 400 rpm, the feeding rate was 5 Hz, and the extrusion temperature zones were set to 170, 170, 175, 180, 180, 175, 170, and 165°C.

[0038] Example 3

[0039] The application of the modified cellulose based on nucleophilic addition in the enhanced HDPE proposed by the present invention comprises the following steps:

[0040] S1: At room temperature, 0.5 kg of CE was placed in 25 kg of DMSO and stirred at 100 rpm / min for 0.5 h to prepare a suspension.

[0041] S2: Under N2 protection, add 2.84kg AOI and 4.26g DBTDL premixed solution to the above suspension, react at 50°C, and mix for 3h. After the reaction is completed, add 37.5kg methanol to generate a precipitate, which is then washed and dried to obtain AOI-CE.

[0042] S3: Weigh 0.3 kg of the above AOI-CE, add 1 kg of HDPE and 4 g of DTBP, and mix at high speed for 1 hour to obtain a masterbatch.

[0043] S4: The masterbatch described in S3 was melt-extruded, the screw speed was 400 rpm, the feeding rate was 5 Hz, and the extrusion temperature zones were set to 170, 170, 175, 180, 180, 175, 170, and 165°C.

[0044] Comparative Example 1

[0045] The preparation method of the enhanced HDPE proposed in this scheme has the following steps:

[0046] S1: Weigh 1 kg of HDPE and 0.3 kg of CE filler and mix them at high speed for 1 hour to prepare a masterbatch.

[0047] S2: The masterbatch described in S1 was melt-extruded, the screw speed was 400 rpm, the feeding rate was 6 Hz, and the extrusion temperature zones were set to 165, 170, 175, 180, 185, 190, 195, 195, 195, 190, 185°C.

[0048] Comparative Example 2

[0049] The preparation method of the enhanced HDPE proposed in this scheme has the following steps:

[0050] S1: At room temperature, 0.5 g of CE was placed in 25 kg of DMSO and stirred at 100 rpm / min for 0.5 h to prepare a suspension.

[0051] S2: Under N2 protection, add 2.84kg AOI and 4.26g DBTDL premixed solution to the above suspension, react at 75°C, and mix for 3h. After the reaction is completed, add 37.5kg methanol to generate a precipitate, which is then washed and dried to obtain AOI-CE.

[0052] S3: Weigh 1 kg of HDPE and 0.3 kg of the above AOI-CE, mix at high speed for 1 hour to obtain a masterbatch.

[0053] S4: The masterbatch described in S3 was melt-extruded, the screw speed was 400 rpm, the feeding rate was 5 Hz, and the extrusion temperature zones were set to 170, 170, 175, 180, 180, 175, 170, and 165°C.

[0054] The present invention conducts mechanical property tests on the samples prepared in Examples 1-3 and Comparative Examples 1-2 and pure HDPE samples, and the results are shown in Table 1. The standards for the tests of flexural strength and flexural modulus are GB / T 9341-2008 "Plastics - Determination of flexural properties"; the standards for the tests of tensile strength and elongation at break are GB / T 1040.1-2006 "Plastics - Determination of tensile properties".

[0055] Table 1 Mechanical properties of samples

[0056]

[0057] As shown in Table 1, the mechanical properties of the HDPE / AOI-CE sample prepared in Example 1 are the best, with a tensile strength of 31.66 MPa, an elongation at break of 670%, and a flexural strength of 26.86 MPa. Overall, the mechanical properties of the untreated CE composite material are enhanced compared with those of pure HDPE, with the tensile strength increasing from 18.35 MPa to 20.28 MPa, an increase of 10.51%, and the flexural strength increasing from 15.51 MPa to 18.65 MPa, an increase of 20.24%. However, the increase in the untreated CE composite material is insufficient compared with the AOI-CE composite material. It can be seen that compared with pure HDPE, the tensile strength of the AOI-CE composite material increased from 18.35 MPa to 31.66 MPa, an increase of 72.53%, and the flexural strength increased from 15.51 MPa to 26.86 MPa, an increase of 73.18%, and the mechanical properties were significantly enhanced. This is because when HDPE is directly blended with CE, unmodified CE will agglomerate in the matrix, while after CE is modified, its compatibility with HDPE increases, enhancing the intermolecular compatibility and improving the mechanical properties of the prepared AOI-CE composite material.

[0058] The water contact angle test was performed on the CE and AOI-CE samples in Example 1. Figure 2 As shown in the figure, the water contact angle of the initial CE at 3 minutes is 25.3°, which has a certain hydrophilicity. After the modification, the water contact angle of AOI-CE at 3 minutes is 59.8°, the water contact angle increases, the hydrophobicity is improved, and the CE can be better compatible with the resin matrix. After the surface modification of CE, the overall structure improves the hydrophobicity, which reduces the agglomeration phenomenon during use, improves the dispersibility with the resin material, and thus the mechanical effect of the composite material is better.

[0059] The present invention performs infrared detection and analysis on the HDPE, CE, AOI-CE and HDPE / AOI-CE samples in Example 1, and the results are as follows: Figure 1 As shown. Figure 1It can be seen that the characteristic peaks of CE functional groups are at 3000–3600 cm -1 There is strong absorbance at 900-1100cm -1 Multiple peaks appeared at 3356 cm-1, which are related to -OH and -C–O–C– vibrations. -1 A sharp peak appears at the position of 1729cm, which is the characteristic peak of carbamate NH. -1 C=O peak appears. It can be concluded that AOI is successfully introduced into the CE structure to obtain modified CE. 1622cm -1 The small peak at represents the C═C stretching vibration of the olefin group in AOI, while this vibration is not found in HDPE / AOI-CE. It can be concluded that the carbon-carbon double bond structure of AOI is broken, and there is an obvious C═O peak. It can be seen that the overall AOI-CE has been grafted onto the HDPE main chain.

[0060] Figure 3 Schematic diagram of the AOI-CE synthesis mechanism proposed by the present invention; Figure 4 Schematic diagram of the preparation mechanism of HDPE / AOI-CE composite material proposed in the present invention. Figure 3 As shown, the present invention utilizes CE and AOI to react chemically under the catalysis of DBTDL, and the hydroxyl groups on the surface of CE react with the isocyanate groups at one end of AOI to generate a carbamate bond. The hydrophilic hydroxyl groups are reduced, thereby weakening the hydrophilicity of CE and improving its application in non-polar or hydrophobic matrices. Figure 2 From the above, the contact angle of CE increased from 29.7° to 55.1° after modification, which changed the surface properties of CE matrix, increased the surface contact angle, and thus improved the compatibility. Figure 4 As shown, in the present invention, DTBP is used as an initiator, which is decomposed into tert-butyl radicals when heated, and the free radicals attack the HDPE macromolecular chain to generate HDPE·, and the AOI-CE modified in the previous step is introduced. The carbon-carbon double bond at the other end of the AOI can undergo a free radical polymerization reaction with HDPE. Thereby, the compatibility of the CE filler and the resin as a whole is achieved, so that the mechanical strength of the composite material is improved. According to the mechanical properties in Table 1, the mechanical strength of the AOI-CE composite material is greater than that of the unmodified CE composite material, the tensile strength increases from 20.28Mpa to 31.66Mpa, and the bending strength increases from 18.65Mpa to 26.86Mpa. It can be obtained that the prepared AOI-CE composite material has good mechanical properties.

Claims

1. A method for preparing modified cellulose based on nucleophilic addition, It is characterized in that The steps are as follows: S1: Under normal temperature, cellulose is placed in dimethyl sulfoxide to prepare a suspension; S2: Under the protection of inert gas, a premixed solution of ethyl isocyanate acrylate and dibutyltin laurate is added to the suspension of S1 to react, and then precipitated, washed and dried to obtain modified cellulose.

2. The method for preparing modified cellulose based on nucleophilic addition according to claim 1, It is characterized in that The concentration of cellulose in S1 is 0.99-2.44 wt %, the stirring speed is 80-100 rpm / min, and the stirring time is 0.5-2 h.

3. The method for preparing modified cellulose based on nucleophilic addition according to claim 1, It is characterized in that The mass ratio of cellulose, ethyl isocyanate acrylate and dibutyltin laurate is 1:5.68-6.25:0.0057-0.

019.

4. The method for preparing modified cellulose based on nucleophilic addition according to claim 1, It is characterized in that The reaction temperature in S2 is 50-85°C and the reaction time is 2-3h.

5. Modified cellulose based on nucleophilic addition prepared by the method according to any one of claims 1 to 4.

6. Use of the modified cellulose based on nucleophilic addition as claimed in claim 5 in reinforced HDPE.

7. The use of the modified cellulose based on nucleophilic addition in reinforced HDPE according to claim 6, It is characterized in that The method comprises the following steps: mixing HDPE, modified cellulose and di-tert-butyl peroxide at high speed and then melt-extruding the mixture.

8. The use of the modified cellulose based on nucleophilic addition in reinforced HDPE according to claim 7, It is characterized in that The mass ratio of HDPE, modified cellulose and di-tert-butyl peroxide is 1:0.10-0.40:0.0010-0.0040.

9. The use of the modified cellulose based on nucleophilic addition in reinforced HDPE according to claim 7, It is characterized in that The high-speed mixing temperature is 30-45°C and the time is 1-2h.

10. The use of the modified cellulose based on nucleophilic addition in reinforced HDPE according to claim 7, It is characterized in that The conditions for melt extrusion were: screw speed of 200-400 rpm, feed rate of 5-7 Hz, and extrusion temperature zones of 170, 170, 175, 180, 180, 175, 170, 165 °C.