Preparation method of low-temperature-resistant ethylene-tetrafluoroethylene copolymer

By introducing low-temperature thermal conductivity additives and controlling reaction conditions into the polymerization kettle, the problem of insufficient low-temperature resistance of ethylene-tetrafluoroethylene copolymer is solved, significantly improving its mechanical and thermal conductivity at low temperatures, and broadening the application field.

CN119019595APending Publication Date: 2024-11-26INNER MONGOLIA FLUORINE TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411080730.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing technology has failed to effectively study and solve the low temperature resistance of ethylene-tetrafluoroethylene copolymers, which limits its application in low temperature environments.

Method used

Polymerization is carried out in a polymerization kettle with a stirrer and heat exchange jacket. The oxygen is removed by introducing high-purity nitrogen, deoxygenated deionized water, solvent and modified monomer, and low-temperature heat-resistant additives such as amino groups are introduced. Multi-walled carbon nanotubes and ferrocene are used to control the reaction temperature and pressure to ensure the progress of the polymerization reaction.

Benefits of technology

The low temperature resistance of ethylene-tetrafluoroethylene copolymer is improved, and its mechanical and thermal conductivity is enhanced, making it have higher tolerance and application potential in low temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides a preparation method of a low-temperature-resistant ethylene-tetrafluoroethylene copolymer, and belongs to the technical field of fluoropolymer preparation. The method comprises the following steps: replacing and removing oxygen in a polymerization kettle with a stirrer and a heat exchange jacket, adding deoxidized deionized water, a solvent and a modified monomer into the polymerization kettle through a pump, starting stirring, heating, introducing tetrafluoroethylene and ethylene to maintain reaction pressure, pumping a low-temperature-resistant heat-conducting auxiliary agent and an initiator, continuously introducing tetrafluoroethylene and ethylene during reaction, and continuously introducing tetrafluoroethylene and ethylene during reaction; and after the reaction is finished, cooling the reaction kettle, and filtering and drying a product to obtain the low-temperature-resistant ethylene-tetrafluoroethylene copolymer. The low-temperature heat-conducting additive prepared by the method can effectively improve the tolerance of the ethylene-tetrafluoroethylene copolymer in a low-temperature environment, and widens the application field of the ethylene-tetrafluoroethylene copolymer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorine-containing polymer preparation, in particular to a method for preparing a low-temperature resistant ethylene-tetrafluoroethylene copolymer. Background Art

[0002] ETFE (F-40) fluoroplastic has the corrosion resistance of polytetrafluoroethylene and the unique strong adhesion to metals, overcoming the non-adhesion defect of polytetrafluoroethylene to metals. In addition, its average linear expansion coefficient is close to that of carbon steel, making ETFE (F-40) an ideal composite material for metals with excellent negative pressure resistance.

[0003] Chinese patent application CN202111612112.9 discloses a preparation method, copolymer and application of ethylene-tetrafluoroethylene copolymer, wherein ethylene and tetrafluoroethylene are used as polymerization monomers, and a fluorine-silicon functional macromolecule containing an olefinic double bond of the formula (I) is polymerized as a third modified monomer; wherein the molar percentages of the three monomers are 70-85% of tetrafluoroethylene monomer, 10-25% of ethylene monomer, and 0.5-5% of the third modified monomer. The preparation method of the present invention is environmentally friendly and has a simple process. The prepared ethylene-tetrafluoroethylene copolymer also has resistance to thermal stress cracking, resistance to low temperatures, and excellent mechanical properties.

[0004] Chinese patent application CN200810138051.5 discloses an ethylene-tetrafluoroethylene copolymer, which is obtained by copolymerizing four monomers: ethylene, tetrafluoroethylene, hexafluoropropylene and 1,2,2-trifluorostyrene. The total molar proportion of ethylene and tetrafluoroethylene in the copolymer is 90-99.9%, and the total molar proportion of the remaining monomers in the copolymer is 0.1-10%.

[0005] Chinese patent application CN110467695B discloses a method for preparing ethylene-tetrafluoroethylene copolymer. The main improvement is that in the process of preparing ethylene-tetrafluoroethylene copolymer by emulsion polymerization using ethylene and tetrafluoroethylene as raw materials, a mixed solution of water and an organic solvent is used as a reaction medium, and a polymerization reaction is carried out under the action of a redox mixed initiator, and the polymerization reaction temperature is 40-55°C; after the polymerization reaction is completed, the obtained polymer is sintered at a temperature of 320-350°C to obtain the obtained copolymer.

[0006] However, the above-mentioned public data do not disclose research on the low temperature resistance of ethylene-tetrafluoroethylene copolymer. In view of this, the present invention provides a method for preparing low temperature resistant ethylene-tetrafluoroethylene copolymer. Summary of the invention

[0007] The object of the present invention is to provide a method for preparing a low-temperature resistant ethylene-tetrafluoroethylene copolymer, so as to prepare an ethylene-tetrafluoroethylene copolymer that can be used resistant to low temperatures.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] A method for preparing a low-temperature resistant ethylene-tetrafluoroethylene copolymer, characterized in that it comprises the following steps:

[0010] Step 1: repeatedly introduce high-purity nitrogen into a polymerization kettle equipped with a stirrer and a heat exchange jacket to remove oxygen from the polymerization kettle;

[0011] Step 2: Add 100-200 parts of deoxygenated deionized water, 2500-3500 parts of solvent and 40-80 parts of modified monomer into the above polymerization kettle through a pump, and start stirring;

[0012] Step 3: The polymerization kettle is heated through the jacket, and a mixed gas 1 of tetrafluoroethylene and ethylene is introduced to the polymerization reaction pressure, and an auxiliary pump pumps in 0.3-2 parts of a low-temperature resistant heat conductive auxiliary agent and 0.1-0.5 parts of an initiator to initiate the polymerization reaction. During the reaction, a mixed gas 2 of tetrafluoroethylene and ethylene is continuously introduced to maintain the polymerization reaction pressure;

[0013] Step 4: After reacting for 2-4 hours, the reaction is completed, the reactor is cooled, the unreacted gas phase monomer is recovered, the polymer dispersion is taken out from the bottom of the polymerization reactor, washed with boiling water, filtered and dried to obtain a low temperature resistant ethylene-tetrafluoroethylene copolymer.

[0014] Furthermore, in the step 1, the oxygen content in the polymerization reactor is required to be no higher than 50 ppm, and the nitrogen content is required to be no higher than 3%.

[0015] Furthermore, in step 2, the solvent is selected from at least one of tert-butyl alcohol, methanol and acetone.

[0016] Furthermore, in the step 2, the reaction temperature of the polymerization reactor is 45-75° C., and the reaction pressure is 3.5-4.2 MPa.

[0017] Furthermore, in step 2, the modified monomer is selected from at least one of hexafluoropropylene, chlorotrifluoroethylene and hexafluoroisobutylene.

[0018] Furthermore, in step 3, the molar ratio of the mixed gas 1 of tetrafluoroethylene and ethylene is 1:0.1-0.5.

[0019] Furthermore, in step 3, the molar ratio of the mixed gas 2 of tetrafluoroethylene and ethylene is 1:0.6-1.2.

[0020] Furthermore, in step 3, the initiator is selected from at least one of ammonium persulfate, potassium persulfate and sodium persulfate.

[0021] Furthermore, the preparation method of the low temperature resistant thermal conductive auxiliary agent in step 3 is:

[0022] Nitrogen is introduced into the reaction container by weight to completely replace the air, 150-200 parts of amino multi-walled carbon nanotubes MWNTs-NH2, 0.05-0.6 parts of 1,1'-diaminoferrocene, 20-30 parts of lanthanum methacrylate, 1000-1500 parts of tetrahydrofuran, and 3-6 parts of tetramethylguanidine are added, and the reaction is carried out at 60-80° C. for 50-120 minutes, filtered, and the product is placed in a vacuum drying oven and dried at room temperature to obtain a low-temperature resistant thermal conductive additive.

[0023] Furthermore, the aminated multi-walled carbon nanotubes MWNTs-NH2 have an outer diameter of 8-15 nm, a length of 50-100 μm, and an amino content of 0.4-1.5 wt%.

[0024] The principle of low temperature resistant additive is:

[0025] MWNTs-NH2 and 1,1'-diaminoferrocene react with lanthanum methacrylate to form amino-acrylic acid groups. Since lanthanum methacrylate has three acrylic acid groups, it can be used as a crosslinker. At the same time, the excess acrylic acid groups can participate in the polymerization of tetrafluoroethylene and ethylene, and introduce ferrocene, MWNTs, and lanthanum complexes into the polymer skeleton.

[0026] Compared with the prior art, the low-temperature resistant ethylene-tetrafluoroethylene copolymer prepared in the embodiment of the present invention has the following beneficial effects:

[0027] 1. Ferrocene is an organic metal compound with a low melting point and high thermal stability, and can be used as a low-temperature modifier for ethylene-tetrafluoroethylene copolymers. MWNTs (multi-walled carbon nanotubes) have excellent thermal conductivity and mechanical properties, and can effectively improve the low-temperature resistance of polymers.

[0028] 2. The introduction of ferrocene and MWNTs can enhance the mechanical properties of ethylene-tetrafluoroethylene copolymers, including tensile strength, compressive strength and wear resistance. Lanthanum complexes can also increase the hardness of polymers to a certain extent, thereby improving their mechanical properties.

[0029] 3.MWNTs have high thermal conductivity and can effectively transfer heat, thereby improving the thermal conductivity of polymers. This is very important for the use of ethylene-tetrafluoroethylene copolymers in high-power electronic devices and microelectronic devices. DETAILED DESCRIPTION

[0030] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0031] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0032] <Example 1>

[0033] A method for preparing a low-temperature resistant ethylene-tetrafluoroethylene copolymer, characterized in that it comprises the following steps:

[0034] Step 1: repeatedly introduce high-purity nitrogen into a polymerization kettle equipped with a stirrer and a heat exchange jacket to remove oxygen from the polymerization kettle;

[0035] Step 2: Add 100 g of deoxygenated deionized water, 2500 g of solvent and 40 g of modified monomer into the above polymerization kettle through a pump, and start stirring;

[0036] Step 3: The polymerization kettle is heated through the jacket, and a mixed gas 1 of tetrafluoroethylene and ethylene is introduced to the polymerization reaction pressure, and an auxiliary pump pumps in 0.3 g of a low-temperature resistant heat conductive auxiliary agent and 0.1 g of an initiator to initiate the polymerization reaction. During the reaction, a mixed gas 2 of tetrafluoroethylene and ethylene is continuously introduced to maintain the polymerization reaction pressure;

[0037] Step 4: After reacting for 2 hours, the reaction is completed, the reactor is cooled, the unreacted gas phase monomer is recovered, the polymer dispersion is taken out from the bottom of the polymerization reactor, washed with boiling water, filtered and dried to obtain a low temperature resistant ethylene-tetrafluoroethylene copolymer.

[0038] In the step 1, the oxygen content in the polymerization reactor is required to be no higher than 50 ppm, and the nitrogen content is required to be no higher than 3%.

[0039] In the step 2, the solvent is selected from tert-butyl alcohol.

[0040] In the step 2, the reaction temperature of the polymerization kettle is 45° C. and the reaction pressure is 4.2 MPa.

[0041] In the step 2, the modified monomer is selected from hexafluoropropylene.

[0042] In step 3, the molar ratio of the mixed gas 1 of tetrafluoroethylene and ethylene is 1:0.1.

[0043] In step 3, the molar ratio of the mixed gas 2 of tetrafluoroethylene and ethylene is 1:0.6.

[0044] In step 3, the initiator is selected from ammonium persulfate.

[0045] The preparation method of the low temperature resistant thermal conductive auxiliary agent in step 3 is:

[0046] Nitrogen was introduced into the reaction container to completely replace the air, and 150 g of amino-modified multi-walled carbon nanotubes MWNTs-NH2, 0.1 g of 1,1'-diaminoferrocene, 20 g of lanthanum methacrylate, 1000 g of tetrahydrofuran, and 3 g of tetramethylguanidine were added. The reaction was carried out at 60° C. for 120 minutes, and the product was filtered. The product was then placed in a vacuum drying oven and dried at room temperature to obtain a low-temperature resistant thermal conductive additive.

[0047] The amino content of the aminated multi-walled carbon nanotubes is 0.4 wt %.

[0048] <Example 2>

[0049] A method for preparing a low-temperature resistant ethylene-tetrafluoroethylene copolymer, characterized in that it comprises the following steps:

[0050] Step 1: repeatedly introduce high-purity nitrogen into a polymerization kettle equipped with a stirrer and a heat exchange jacket to remove oxygen from the polymerization kettle;

[0051] Step 2: Add 150 g of deoxygenated deionized water, 3000 g of solvent and 60 g of modified monomer into the above polymerization kettle through a pump, and start stirring;

[0052] Step 3: The polymerization kettle is heated through the jacket, and a mixed gas 1 of tetrafluoroethylene and ethylene is introduced to the polymerization reaction pressure, and an auxiliary pump pumps in 1.2 g of a low-temperature resistant heat conductive auxiliary agent and 0.3 g of an initiator to initiate the polymerization reaction. During the reaction, a mixed gas 2 of tetrafluoroethylene and ethylene is continuously introduced to maintain the polymerization reaction pressure;

[0053] Step 4: After reacting for 3 hours, the reaction is completed, the reactor is cooled, and the unreacted gas phase monomer is recovered. The polymer dispersion is taken out from the bottom of the polymerization reactor, washed with boiling water, filtered, and dried to obtain a low-temperature resistant ethylene-tetrafluoroethylene copolymer.

[0054] In the step 1, the oxygen content in the polymerization reactor is required to be no higher than 50 ppm, and the nitrogen content is required to be no higher than 3%.

[0055] In the step 2, the solvent is selected from methanol.

[0056] In the step 2, the reaction temperature of the polymerization kettle is 55° C. and the reaction pressure is 3.9 MPa.

[0057] In the step 2, the modified monomer is selected from chlorotrifluoroethylene.

[0058] In step 3, the molar ratio of the mixed gas 1 of tetrafluoroethylene and ethylene is 1:0.3.

[0059] The molar ratio of the mixed gas 2 of tetrafluoroethylene and ethylene in step 3 is 1:0.9.

[0060] In step 3, the initiator is selected from potassium persulfate.

[0061] The preparation method of the low temperature resistant thermal conductive auxiliary agent in step 3 is:

[0062] Nitrogen was introduced into the reaction container to completely replace the air, and 175 g of amino-modified multi-walled carbon nanotubes MWNTs-NH2, 0.3 g of 1,1'-diaminoferrocene, 25 g of lanthanum methacrylate, 1250 g of tetrahydrofuran, and 4.5 g of tetramethylguanidine were added. The mixture was reacted at 70° C. for 85 minutes, filtered, and the product was dried in a vacuum drying oven at room temperature to obtain a low-temperature resistant thermal conductive additive.

[0063] The amino content of the aminated multi-walled carbon nanotubes is 0.9 wt %.

[0064] <Example 3>

[0065] A method for preparing a low-temperature resistant ethylene-tetrafluoroethylene copolymer, characterized in that it comprises the following steps:

[0066] Step 1: repeatedly introduce high-purity nitrogen into a polymerization kettle equipped with a stirrer and a heat exchange jacket to remove oxygen from the polymerization kettle;

[0067] Step 2: Add 200 g of deoxygenated deionized water, 3500 g of solvent and 80 g of modified monomer into the above polymerization kettle through a pump, and start stirring;

[0068] Step 3: The polymerization kettle is heated through the jacket, and a mixed gas 1 of tetrafluoroethylene and ethylene is introduced to the polymerization reaction pressure, and an auxiliary pump pumps in 2g of a low-temperature resistant heat conductive auxiliary agent and 0.5g of an initiator to initiate the polymerization reaction. During the reaction, a mixed gas 2 of tetrafluoroethylene and ethylene is continuously introduced to maintain the polymerization reaction pressure;

[0069] Step 4: After 4 hours of reaction, the reaction is completed, the reactor is cooled, and the unreacted gas phase monomer is recovered. The polymer dispersion is taken out from the bottom of the polymerization reactor, washed with boiling water, filtered, and dried to obtain a low-temperature resistant ethylene-tetrafluoroethylene copolymer.

[0070] In the step 1, the oxygen content in the polymerization reactor is required to be no higher than 50 ppm, and the nitrogen content is required to be no higher than 3%.

[0071] In step 2, the solvent is selected from at least one of tert-butyl alcohol, methanol and acetone.

[0072] In the step 2, the reaction temperature of the polymerization kettle is 75° C. and the reaction pressure is 3.5 MPa.

[0073] In the step 2, the modified monomer is selected from hexafluoroisobutylene.

[0074] In step 3, the molar ratio of the mixed gas 1 of tetrafluoroethylene and ethylene is 1:0.5.

[0075] In the step 3, the molar ratio of the mixed gas 2 of tetrafluoroethylene and ethylene is 1:1.2.

[0076] In step 3, the initiator is selected from sodium persulfate.

[0077] The preparation method of the low temperature resistant thermal conductive auxiliary agent in step 3 is:

[0078] Nitrogen was introduced into the reaction container to completely replace the air, and 200 g of amino-modified multi-walled carbon nanotubes MWNTs-NH2, 0.6 g of 1,1'-diaminoferrocene, 30 g of lanthanum methacrylate, 1500 g of tetrahydrofuran, and 6 g of tetramethylguanidine were added. The reaction was carried out at 80° C. for 50 minutes, and the product was filtered. The product was then placed in a vacuum drying oven and dried at room temperature to obtain a low-temperature resistant thermal conductive additive.

[0079] The amino content of the aminated multi-walled carbon nanotubes is 1.5 wt %.

[0080] <Comparative Example 1>

[0081] A method for preparing a low-temperature resistant ethylene-tetrafluoroethylene copolymer, characterized in that it comprises the following steps:

[0082] Step 1: repeatedly introduce high-purity nitrogen into a polymerization kettle equipped with a stirrer and a heat exchange jacket to remove oxygen from the polymerization kettle;

[0083] Step 2: Add 100 g of deoxygenated deionized water, 2500 g of solvent and 40 g of modified monomer into the above polymerization kettle through a pump, and start stirring;

[0084] Step 3: The polymerization reactor is heated through the jacket, and a mixed gas 1 of tetrafluoroethylene and ethylene is introduced to the polymerization reaction pressure, and an auxiliary pump pumps 0.1 g of initiator to initiate the polymerization reaction. During the reaction, a mixed gas 2 of tetrafluoroethylene and ethylene is continuously introduced to maintain the polymerization reaction pressure;

[0085] Step 4: After reacting for 2 hours, the reaction is completed, the reactor is cooled, the unreacted gas phase monomer is recovered, the polymer dispersion is taken out from the bottom of the polymerization reactor, washed with boiling water, filtered and dried to obtain a low temperature resistant ethylene-tetrafluoroethylene copolymer.

[0086] In the step 1, the oxygen content in the polymerization reactor is required to be no higher than 50 ppm, and the nitrogen content is required to be no higher than 3%.

[0087] In the step 2, the solvent is selected from tert-butyl alcohol.

[0088] In the step 2, the reaction temperature of the polymerization kettle is 45° C. and the reaction pressure is 4.2 MPa.

[0089] In the step 2, the modified monomer is selected from hexafluoropropylene.

[0090] In step 3, the molar ratio of the mixed gas 1 of tetrafluoroethylene and ethylene is 1:0.1.

[0091] In step 3, the molar ratio of the mixed gas 2 of tetrafluoroethylene and ethylene is 1:0.6.

[0092] In step 3, the initiator is selected from ammonium persulfate.

[0093] <Comparative Example 2>

[0094] A method for preparing a low-temperature resistant ethylene-tetrafluoroethylene copolymer, characterized in that it comprises the following steps:

[0095] Step 1: repeatedly introduce high-purity nitrogen into a polymerization kettle equipped with a stirrer and a heat exchange jacket to remove oxygen from the polymerization kettle;

[0096] Step 2: Add 100 g of deoxygenated deionized water, 2500 g of solvent and 40 g of modified monomer into the above polymerization kettle through a pump, and start stirring;

[0097] Step 3: The polymerization kettle is heated through the jacket, and a mixed gas 1 of tetrafluoroethylene and ethylene is introduced to the polymerization reaction pressure, and an auxiliary pump pumps in 0.3 g of a low-temperature resistant heat conductive auxiliary agent and 0.1 g of an initiator to initiate the polymerization reaction. During the reaction, a mixed gas 2 of tetrafluoroethylene and ethylene is continuously introduced to maintain the polymerization reaction pressure;

[0098] Step 4: After reacting for 2 hours, the reaction is completed, the reactor is cooled, the unreacted gas phase monomer is recovered, the polymer dispersion is taken out from the bottom of the polymerization reactor, washed with boiling water, filtered and dried to obtain a low temperature resistant ethylene-tetrafluoroethylene copolymer.

[0099] In the step 1, the oxygen content in the polymerization reactor is required to be no higher than 50 ppm, and the nitrogen content is required to be no higher than 3%.

[0100] In the step 2, the solvent is selected from tert-butyl alcohol.

[0101] In the step 2, the reaction temperature of the polymerization kettle is 45° C. and the reaction pressure is 4.2 MPa.

[0102] In the step 2, the modified monomer is selected from hexafluoropropylene.

[0103] In step 3, the molar ratio of the mixed gas 1 of tetrafluoroethylene and ethylene is 1:0.1.

[0104] In step 3, the molar ratio of the mixed gas 2 of tetrafluoroethylene and ethylene is 1:0.6.

[0105] In step 3, the initiator is selected from ammonium persulfate.

[0106] The preparation method of the low temperature resistant thermal conductive auxiliary agent in step 3 is:

[0107] Nitrogen was introduced into the reaction container to completely replace the air, and 150 g of amino-modified multi-walled carbon nanotubes MWNTs-NH2, 20 g of lanthanum methacrylate, 1000 g of tetrahydrofuran, and 3 g of tetramethylguanidine were added. The reaction was carried out at 60° C. for 120 minutes, and the product was filtered. The product was then placed in a vacuum drying oven and dried at room temperature to obtain a low-temperature resistant thermal conductive additive.

[0108] The amino content of the aminated multi-walled carbon nanotubes is 0.4 wt %.

[0109] <Comparative Example 3>

[0110] A method for preparing a low-temperature resistant ethylene-tetrafluoroethylene copolymer, characterized in that it comprises the following steps:

[0111] Step 1: repeatedly introduce high-purity nitrogen into a polymerization kettle equipped with a stirrer and a heat exchange jacket to remove oxygen from the polymerization kettle;

[0112] Step 2: Add 100 g of deoxygenated deionized water, 2500 g of solvent and 40 g of modified monomer into the above polymerization kettle through a pump, and start stirring;

[0113] Step 3: The polymerization kettle is heated through the jacket, and a mixed gas 1 of tetrafluoroethylene and ethylene is introduced to the polymerization reaction pressure, and an auxiliary pump pumps in 0.3 g of a low-temperature resistant heat conductive auxiliary agent and 0.1 g of an initiator to initiate the polymerization reaction. During the reaction, a mixed gas 2 of tetrafluoroethylene and ethylene is continuously introduced to maintain the polymerization reaction pressure;

[0114] Step 4: After reacting for 2 hours, the reaction is completed, the reactor is cooled, the unreacted gas phase monomer is recovered, the polymer dispersion is taken out from the bottom of the polymerization reactor, washed with boiling water, filtered and dried to obtain a low temperature resistant ethylene-tetrafluoroethylene copolymer.

[0115] In the step 1, the oxygen content in the polymerization reactor is required to be no higher than 50 ppm, and the nitrogen content is required to be no higher than 3%.

[0116] In the step 2, the solvent is selected from tert-butyl alcohol.

[0117] In the step 2, the reaction temperature of the polymerization kettle is 45° C. and the reaction pressure is 4.2 MPa.

[0118] In the step 2, the modified monomer is selected from hexafluoropropylene.

[0119] In step 3, the molar ratio of the mixed gas 1 of tetrafluoroethylene and ethylene is 1:0.1.

[0120] In step 3, the molar ratio of the mixed gas 2 of tetrafluoroethylene and ethylene is 1:0.6.

[0121] In step 3, the initiator is selected from ammonium persulfate.

[0122] The preparation method of the low temperature resistant thermal conductive auxiliary agent in step 3 is:

[0123] Nitrogen was introduced into the reaction container to completely replace the air, 150 g of amino-modified multi-walled carbon nanotubes MWNTs-NH2, 0.1 g of 1,1'-diaminoferrocene, 1000 g of tetrahydrofuran, and 3 g of tetramethylguanidine were added, and the mixture was reacted at 60° C. for 120 minutes. The mixture was filtered and the product was dried in a vacuum drying oven at room temperature to obtain a low-temperature resistant thermal conductive additive.

[0124] The amino content of the aminated multi-walled carbon nanotubes is 0.4 wt %.

[0125] Example results:

[0126] Low temperature resistance test method: The ethylene-tetrafluoroethylene copolymer test specimen is placed at -60℃ in air atmosphere for 96 hours, and then the mechanical strength test is carried out at room temperature. The mechanical strength test method of ethylene-tetrafluoroethylene copolymer refers to GB / T1040.1.

[0127] Table 1 Test results

[0128]

[0129]

[0130] It can be seen from the above specific implementation scheme that the low-temperature thermal conductive additive added in the embodiment of the method can effectively improve the tolerance of ethylene-tetrafluoroethylene copolymer in low temperature environment, and broaden the application field of ethylene-tetrafluoroethylene copolymer.

[0131] The above are only embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing a low-temperature resistant ethylene-tetrafluoroethylene copolymer, It is characterized in that The steps include: Step 1: repeatedly introduce high-purity nitrogen into a polymerization kettle equipped with a stirrer and a heat exchange jacket to remove oxygen from the polymerization kettle; Step 2: Add 100-200 parts of deoxygenated deionized water, 2500-3500 parts of solvent and 40-80 parts of modified monomer into the above polymerization kettle through a pump, and start stirring; Step 3: The polymerization kettle is heated through the jacket, and a mixed gas 1 of tetrafluoroethylene and ethylene is introduced to the polymerization reaction pressure, and an auxiliary pump pumps in 0.3-2 parts of a low-temperature resistant heat conductive auxiliary agent and 0.1-0.5 parts of an initiator to initiate the polymerization reaction. During the reaction, a mixed gas 2 of tetrafluoroethylene and ethylene is continuously introduced to maintain the polymerization reaction pressure; Step 4: After reacting for 2-4 hours, the reaction is completed, the reactor is cooled, the unreacted gas phase monomer is recovered, the polymer dispersion is taken out from the bottom of the polymerization reactor, washed with boiling water, filtered and dried to obtain a low temperature resistant ethylene-tetrafluoroethylene copolymer.

2. A method for preparing a low temperature resistant ethylene-tetrafluoroethylene copolymer according to claim 1, It is characterized in that In the step 1, the oxygen content in the polymerization reactor is required to be no higher than 50 ppm, and the nitrogen content is required to be no higher than 3%.

3. A method for preparing a low temperature resistant ethylene-tetrafluoroethylene copolymer according to claim 1, It is characterized in that In step 2, the solvent is selected from at least one of tert-butyl alcohol, methanol and acetone.

4. A method for preparing a low temperature resistant ethylene-tetrafluoroethylene copolymer according to claim 1, It is characterized in that In the step 2, the reaction temperature of the polymerization kettle is 45-75° C., and the reaction pressure is 3.5-4.2 MPa.

5. A method for preparing a low temperature resistant ethylene-tetrafluoroethylene copolymer according to claim 1, It is characterized in that In the step 2, the modified monomer is selected from at least one of hexafluoropropylene, chlorotrifluoroethylene and hexafluoroisobutylene.

6. A method for preparing a low temperature resistant ethylene-tetrafluoroethylene copolymer according to claim 1, It is characterized in that In step 3, the molar ratio of the mixed gas 1 of tetrafluoroethylene and ethylene is 1:0.1-0.

5.

7. The method for preparing a low temperature resistant ethylene-tetrafluoroethylene copolymer according to claim 1, It is characterized in that In the step 3, the molar ratio of the mixed gas 2 of tetrafluoroethylene and ethylene is 1:0.6-1.

2.

8. The method for preparing a low temperature resistant ethylene-tetrafluoroethylene copolymer according to claim 1, It is characterized in that In step 3, the initiator is selected from at least one of ammonium persulfate, potassium persulfate and sodium persulfate.

9. The method for preparing a low temperature resistant ethylene-tetrafluoroethylene copolymer according to claim 1, It is characterized in that The preparation method of the low temperature resistant thermal conductive auxiliary agent in step 3 is: Nitrogen was introduced into the reaction vessel to completely replace the air, and 150-200 parts by weight of amino-modified multi-walled carbon nanotubes MWNTs-NH 2 , 0.05-0.6 parts of 1,1'-diaminoferrocene, 20-30 parts of lanthanum methacrylate, 1000-1500 parts of tetrahydrofuran, 3-6 parts of tetramethylguanidine, react at 60-80°C for 50-120 minutes, filter, and then place the product in a vacuum drying oven and dry at room temperature to obtain a low-temperature resistant thermal conductive additive.

10. A method for preparing a low temperature resistant ethylene-tetrafluoroethylene copolymer according to claim 9, It is characterized in that The amino-modified multi-walled carbon nanotubes MWNTs-NH 2 The outer diameter is 8-15nm, the length is 50-100μm, and the amino content is 0.4-1.5wt%.

Citation Information

Patent Citations

  • Ethylene-tetrafluoroethylene copolymer

    CN101302263A

  • An ethylene-tetrafluoroethylene copolymer and its preparation method

    CN110467695B

  • Preparation method of ethylene-tetrafluoroethylene copolymer, copolymer and application thereof

    CN114230706A