Ternary hydrocarbon rubber, preparation method thereof and application of ternary hydrocarbon rubber in inner tube rubber material

By using polyethylene-propylene-butene ternary rubber with high alkyl content (EPBR), the problem of insufficient adhesive roller and airtightness of butyl rubber during processing is solved, forming a stable vulcanization network, and improving the airtightness of the inner tube and physical and mechanical properties make up for the shortcomings in the prior art.

CN119019606AActive Publication Date: 2024-11-26CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310594183.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-26
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

In the existing inner tube materials, butyl rubber has difficulty in sticking rollers and lower sheets during processing and mixing. When adding ethylene propylene rubber, the content of methyl on the side of the molecular chain is low, the airtightness decreases, and sulfurization. Rate mismatch, physical and mechanical performance insufficient.

Method used

Polyethylene-propylene-butene ternary rubber (EPBR) is used, which contains a high proportion of side alkyl groups, hinders the thermal movement of the molecular chain, forms a stable and uniform vulcanization network, matches the co-vulcanization rate of butyl rubber, and improves airtightness. and physical and mechanical properties, and control molecular structure and vulcanization effects through specific preparation methods and process conditions.

Benefits of technology

It achieves excellent airtightness, low deformation, high resilience and anti-aging properties, avoiding the problem of later softening and swelling of butyl rubber, and improving the physical and mechanical properties and processing performance of the inner tube.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019606A_ABST
    Figure CN119019606A_ABST
Patent Text Reader

Abstract

The invention discloses ternary hydrocarbon rubber as well as a preparation method and application thereof in an inner tube rubber material, and belongs to the technical field of high polymer materials. The ternary hydrocarbon rubber has the following structural expression: # imgabs0 #, wherein R1 and R2 are independently selected from hydrogen or C1-C3 alkyl groups; r3 and R4 are independently selected from hydrogen, C1-C3 alkyl groups or vinyl groups; ar is phenyl or substituted phenyl; x, n, y, m and z are all greater than or equal to 0, the sum of x, n, y and m is greater than 0, and (x + y + z) / (m + n) = 49-99; and the obtained vulcanized rubber has the characteristics of good air tightness, lasting resistance, excellent physical and mechanical properties, good heat resistance, no softening, no stickiness, no swelling, easiness in processing and molding and the like in the later use period.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a ternary hydrocarbon rubber, in particular to a polyethylene-propylene-butene ternary rubber (EPBR), and also to a preparation method and application of the ternary rubber in inner tube rubber, belonging to the technical field of new rubber materials. Background Art

[0002] The ethylene propylene diene monomer (EPDM) in the prior art usually has 30-70% ethylene segments. As the ethylene segments increase, the strength of the raw rubber increases, the elongation at break decreases, and the relative permanent deformation after breaking increases. Its operating temperature is -60-125°C, and it has good weather resistance, stable chemical resistance, excellent dielectric properties, low density, and good product shape repeatability. It has been widely used in automotive products and home appliances, and has been widely used in cable, sealing, and shock-absorbing material industries. In addition, commercially available ethylene propylene diene monomers such as EPDM4045M and EPDM4770P are usually copolymerized with ethylene and propylene as the third monomer, and the side olefin groups are vulcanized faster than the double bonds on the main chain. As an airtight inner tube butyl rubber (IIR), the main chain of the molecule contains isoprene and isobutylene copolymerized to form a double bond on the main chain, which has a relatively slow vulcanization speed. Due to the poor processing performance and easy sticking to the roller of IIR, 25-30% EPDM is usually added to the IIR inner tube formula to improve the processing performance, but the vulcanization speeds of the two do not match, resulting in the physical properties of the vulcanized rubber not reaching the best. In the automobile tire industry, EPDM cannot be promoted in the tire body and tread parts where a large amount of materials are used, because EPDM has poor compatibility with other rubbers, and only a small amount of EPDM is used in the inner tube, white sidewall, tire strip and other parts.

[0003] The use of EPDM rubber and other rubbers is a very large field. The use of EPDM rubber and other rubbers can complement each other in performance, improve the process and reduce costs. However, due to the different affinity of various compounding agents for different polymers, the co-vulcanization depends on the cross-linking efficiency of each polymer. It is impossible to achieve molecular compatibility when different polymers are used together, resulting in uneven phase separation. This uneven distribution of compounding agents has a significant impact on the performance of EPDM rubber. EPDM rubber and butyl rubber have good compatibility and co-vulcanization, and the physical and mechanical properties of the two rubbers are additive. Butyl rubber can improve the air tightness of EPDM rubber, improve the tearing and sound insulation properties; while EPDM rubber improves the ozone resistance and aging resistance of butyl rubber, improves the extruded surface gloss of butyl rubber, and improves the anti-deformation performance of semi-finished products when parked. EPDM rubber, like IIR, is a hydrocarbon rubber and the two have good compatibility. Usually, 30% EPDM is added to the formula of inner tubes made mainly of IIR to complement and improve the process and reduce the processing performance of IIR in terms of roller sticking.

[0004] The patent (CN108395584A) discloses a formula for automobile tire inner tubes composed of natural rubber, solution-polymerized styrene-butadiene rubber, butyl reclaimed rubber, fillers and reinforcing agents, softeners, activators, antioxidants and vulcanizers / accelerators, and a preparation method thereof. The combined use of natural rubber, solution-polymerized styrene-butadiene rubber and butyl reclaimed rubber can improve the mechanical properties and physical and mechanical properties of the inner tube, so that the tire has good heat resistance, cold resistance, pressure resistance, wear resistance and flex resistance, can meet the daily use requirements of automobile tires, and extend the service life of the tire. However, the inner tube made by this method contains NR and SSBR with high unsaturation, and there will be great deficiencies in its air tightness and anti-aging. The patent (CN108395634A) involves a new type of automobile inner tube and a preparation method thereof, which is mainly composed of polyurethane PU, butyl rubber, EPDM rubber, CaSO 4 Whiskers, carbon fiber, glass fiber, accelerator CZ, antioxidant 6PPD, antioxidant TMQ, stabilizer HS-80, vulcanized rubber, vulcanization accelerator, compound intercalation modified powder, physical plasticizer WP-1. It has the advantages of good elasticity, good comfort, improved pressure resistance and various mechanical strengths; CaSO 4 The use of whiskers, carbon fibers and glass fibers can significantly enhance the various mechanical properties of the inner tube, thereby obtaining a new type of automobile inner tube with high green environmental protection safety performance and good performance. The formula of the rubber composite material for tire inner tube involved in the patent (CN 105462013A) is: 60-80 reclaimed rubber, 5-10 polyurethane resin, 2-4 rosin glycerol ester, 10-15 coal gangue powder, 20-30 montmorillonite, 6-8 rosin, 2-4 butyl acrylate, 0.15-0.25 potassium persulfate, 1-2 hydroxyethyl cellulose, 0.15-0.25 sodium dodecyl sulfate, 1-2 zinc stearate, 1-2 sodium petroleum sulfonate, 5-10 composite additives, 1-2 sulfur. However, the mechanical properties of the inner tube made by this method cannot be guaranteed in theory. Patent (CN103819819A) discloses an EPDM / montmorillonite nanocomposite material, which is mixed with EPDM, nano-montmorillonite and dicumyl peroxide in a weight ratio of 100:1 to 10:2 to 5. The raw materials are mixed evenly according to a certain weight ratio, added to an open mixer or an internal mixer for mixing, and then placed on a flat vulcanizer for tableting, and finally a EPR / MMT nanocomposite material with good reinforcement effect and uniform dispersion is obtained. The composite material is in a peeled sheet state, and after being modified by nano-montmorillonite, the tensile strength and elongation at break of the EPDM matrix are significantly improved.

[0005] In (“Research on Butyl Rubber / EPDM Rubber Inner Tube and Realization of Lightweighting”, Synthetic Rubber Industry, Issue 6, 1993) and (“Using EPDM Rubber and Butyl Rubber to Make Inner Tube”, Tire Industry, Issue 004, 1994), the study on the use of butyl rubber and an appropriate amount of EPDM rubber to make inner tubes not only maintains the inner tube's long-lasting physical and mechanical properties and excellent air tightness, but also solves the problems of butyl rubber becoming soft, sticky and swollen in the later period of use, and achieves good corporate economic benefits and social benefits. At the same time, in (“Application of EPDM Recycled Rubber in Butyl Rubber / EPDM Rubber Inner Tube Rubber”, Rubber Science and Technology, Issue 008, 2012), the study on the use of 27.2 parts of EPDM recycled rubber in inner tube rubber can significantly improve the joint strength and processing performance, improve the softening problem of finished inner tube in the later period of use, improve the aging resistance of finished inner tube, and reduce production costs.

[0006] In summary, the materials used in the existing inner tube manufacturing are all diene rubbers, mainly butyl rubber and EPDM rubber compounded with fillers, and the technology of using polyethylene-propylene-butene rubber to prepare inner tubes has not been reported in the literature. Summary of the invention

[0007] In the prior art, the rubber used for inner tubes is mainly butyl rubber, and single butyl rubber has problems such as sticking to rollers and difficulty in unrolling during processing and mixing. When EPDM rubber is added to the inner tube formula to improve its processing performance, due to the low propylene content and high crystallinity of EPDM rubber, the content of side methyl groups in the molecular chain is low, and the hindrance of the molecules in thermal motion is small, resulting in reduced air tightness of the inner tube. In addition, the vulcanization rate of the side olefin groups in the existing EPDM rubber molecules is much higher than the double bonds in the main chain of the butyl rubber molecules, resulting in defects such as mismatched co-vulcanization rates or uneven crosslinking density.

[0008] The first object of the present invention is to provide a ternary hydrocarbon rubber, which contains a relatively high proportion of side alkyl groups. The steric hindrance effect of the side alkyl groups can hinder the thermal movement of the molecular chain, so that it exhibits excellent air tightness, and also has the characteristics of low crystallinity, low deformation and high resilience, and the double bonds in the molecular chain mainly exist in straight chains and side branches, which can form a stable and uniform vulcanization network by co-vulcanization with the straight chain double bonds in the butyl rubber molecular chain. The vulcanized rubber has excellent comprehensive physical and mechanical properties, and has excellent anti-aging performance after vulcanization. The aging mechanism is the coexistence of degradation aging and cross-linking aging, and the hardness shows a trend of slowly increasing, which makes up for the disadvantages of softening, stickiness and swelling in the later aging process of the existing butyl rubber in the use process, and is particularly suitable for inner tube rubber.

[0009] The second object of the present invention is to provide a method for preparing a ternary hydrocarbon rubber, which is simple, low-cost, can be produced using existing mature processes, and is easy to control and industrialize.

[0010] The third object of the present invention is to provide an application of a ternary hydrocarbon rubber, which is mixed with butyl rubber for vulcanization and molding. The obtained vulcanized rubber has good airtightness, durability, excellent physical and mechanical properties, good heat resistance, does not soften, become sticky or swell in the later stage of use, and is easy to process and mold.

[0011] In order to achieve the above technical objectives, the present invention provides a ternary hydrocarbon rubber having the following structural expression:

[0012]

[0013] in,

[0014] R 1 and R 2 independently selected from hydrogen or C 1 ~C 3 The alkyl group;

[0015] R 3 and R 4 independently selected from hydrogen, C 1 ~C 3 Alkyl or vinyl;

[0016] Ar is phenyl or substituted phenyl;

[0017] x, n, y, m and z are the degree of polymerization, x, n, y, m and z are all greater than or equal to 0, and the sum of x, n, y and m is greater than 0, (x+y+z) / (m+n)=49-99;

[0018] The unsaturation degree of the ternary hydrocarbon rubber by iodine value method is 1.0-2.0%, and the mass proportion of the side alkyl chain is not less than 65%.

[0019] The ternary hydrocarbon rubber provided by the present invention is specially polyethylene-propylene-butylene ternary rubber (hereinafter referred to as EPBR), and its main chain is mainly an alkyl chain, and its main chain structure is similar to butyl rubber, and both have good compatibility. EPBR includes a relatively high side alkyl group at the same time, and the steric effect of the side alkyl group can hinder the molecular chain thermal motion, so that it embodies excellent air tightness, and each polymerized unit in EPBR presents random distribution, and can effectively reduce the crystallinity of the polymer, so that it also has the characteristics of low crystallinity, low deformation and high resilience. And the EPBR molecular chain also includes highly active side branches and a small amount of straight-chain vinyl at the same time, and can be co-vulcanized with the straight-chain double bond in the butyl rubber molecular chain to form a stable and uniform vulcanization network, so that the vulcanized rubber has excellent comprehensive physical and mechanical properties, and EPBR and the straight-chain double bond in the butyl rubber molecular chain carry out co-vulcanization rate matching, and the curing time is short, and the vulcanization effect is good, and the physical and mechanical properties are good after vulcanization.

[0020] The unsaturation in the EPBR molecule provided by the present invention should be controlled within an appropriate range. If the unsaturation is too high, the vulcanization speed is fast; if the unsaturation is too low, the vulcanization speed is slow. Since the unsaturation of butyl rubber is usually 1.0-2.0%, in order to ensure better coordination between EPBR and butyl rubber and form a common uniform crosslinking, the unsaturation in the preferred EPBR molecule is 1.0-2.0%, which is more suitable. It should be noted that the unsaturation involved in the above is the unsaturation measured by the iodine value method, which is mainly the unsaturation shown by the olefin group, and does not include the unsaturation of the benzene ring.

[0021] The mass content of the side alkyl groups in the EPBR molecules provided by the present invention is not less than 65%, mainly to ensure that after the EPBR and the butyl rubber are vulcanized and cross-linked, there are enough or larger side alkyl groups in the network molecules, so that the vulcanized rubber can be ensured to have good air tightness, and the gas molecules of the vulcanized rubber can be prevented from escaping from the inner tube during the thermal motion. The more side alkyl groups have a blocking and shielding effect on the thermal motion of the gas molecules, thereby ensuring the air tightness of the compressed air in the inner tube, and at the same time, the crystallinity of the EPBR can be reduced.

[0022] As a preferred solution, R 1 and R 2 Selected from C 1 ~C 3 When the alkyl group is a linear alkyl group, the alkyl group may be a branched alkyl group, for example, a methyl group, an ethyl group, a propyl group, an isopropyl group, and the like.

[0023] As a preferred embodiment, Ar can be selected as phenyl, or phenyl containing conventional substituents, such as methyl, ethyl, methoxy and the like.

[0024] As a preferred solution, R 3 and R 4 Selected from C1 ~C 3 When the alkyl group is a linear alkyl group, the alkyl group may be a branched alkyl group, for example, a methyl group, an ethyl group, a propyl group, an isopropyl group, and the like.

[0025] As a preferred solution, the Mooney viscosity ML of the ternary hydrocarbon rubber is 100℃ =40~55, molecular mass distribution index M w / M n The EPBR of the present invention has a wide molecular weight distribution and a low crystallinity, which can give it good processing performance and high filling performance, make up for the shortcomings of butyl rubber being sticky and sticky to the roller during mixing, and improve the mixing, processing and vulcanization molding of the composite material.

[0026] The present invention also provides a method for preparing a ternary hydrocarbon rubber, which comprises heating a polymerization solution system containing a structure regulator to a temperature required for initiating polymerization, continuously and evenly adding olefin monomers and alkyl lithium to initiate and carry out a polymerization reaction, and immediately adding divinylbenzene to continue the polymerization reaction after the addition of the olefin monomers and the alkyl lithium to obtain a polymer glue solution; firstly adding alkyl lithium to the polymer glue solution and hydrogenating it for activation, and then adding a hydrogenation catalyst to carry out a catalytic hydrogenation reaction to obtain the polymer glue solution.

[0027] As a preferred solution, the structure regulator includes at least one of difunctional ethers such as tetrahydrofurfuryl alcohol ethyl ether, ditetrahydrofurfuryl propane, tetrahydrofurfuryl alcohol butyl ether and tetrahydrofurfuryl alcohol hexyl ether.

[0028] As a more preferred solution, the concentration of the structure regulator in the polymerization solution system is 200-260 mg / kg solvent.

[0029] The preferred structure regulator and dosage can adjust the content of 1,2-polymerization or 3,4-polymerization units of the conjugated diene monomer within an appropriate ratio range, thereby adjusting the content of the side alkyl group and the side vinyl group.

[0030] As a preferred embodiment, the olefin monomer includes a conjugated diene monomer, or a conjugated diene monomer and an aromatic vinyl monomer;

[0031] The conjugated diene monomers include

[0032] The aromatic vinyl monomers include

[0033] Among them, R 5 Selected from hydrogen, C 1 ~C 3 Ar is selected from phenyl or substituted phenyl.

[0034] The most preferred olefin monomer is at least one of butadiene, isoprene, piperylene, 1,3,5-hexatriene, styrene, and p-alkylstyrene.

[0035] As a preferred solution, the olefin monomer and alkyl lithium are continuously and uniformly added to the polymerization solution system within 30 to 40 minutes. The alkyl lithium is commonly n-butyl lithium. The amount of alkyl lithium added relative to the olefin monomer (or polymer) is 8 to 12 mmol / kg.

[0036] As a preferred solution, the initiation temperature of the polymerization reaction is 50-55°C, and the maximum temperature does not exceed 65°C.

[0037] As a preferred solution, the polymerization reaction is continued for 12 to 20 minutes after the divinylbenzene is added.

[0038] As a preferred solution, the conditions for hydrogenation activation are: the amount of alkyl lithium added to the polymer glue is 10-15 mmol / kg, the temperature is 50-80°C, the hydrogen pressure is 10-13 bar, and the activation time is 5-15 min.

[0039] As a preferred solution, the conditions for the catalytic hydrogenation reaction are: using dimethyl phthalate and / or methyl o-toluate as co-catalysts, dicyclopentadiene titanium dichloride as the main catalyst, the hydrogen pressure is 13-15 bar, the temperature is 70-95° C., and the hydrogenation end point is that the polymer unsaturation is 1.0-2.0%.

[0040] As a preferred solution, the amount of the main catalyst added to the polymer glue is 3.0-4.0 mmol / kg, and the molar ratio of the main catalyst to the co-catalyst is 7-10. The preferred dicyclopentadiene titanium dichloride catalyst system can effectively control the degree of hydrogenation or unsaturation of the polymer glue, and it is not easy to hydrogenate all the double bonds in the polymer glue. At the same time, for the polymer chain segments containing conjugated dienes with more than 5 carbon atoms with a certain steric effect, it will lead to hydrogenation selectivity, thereby ensuring that the hydride has a suitable degree of unsaturation. If the common nickel-based catalyst is used for hydrogenation, it is difficult to remove the catalyst and the cost is high. The polymer is easily completely hydrogenated into a saturated carbon-carbon chain, and the vulcanization crosslinking point is lost.

[0041] As a preferred solution, the amount of divinylbenzene added relative to the conjugated diene monomer is 0.50-0.75 g / kg. By introducing a small amount of divinylbenzene, the molecular weight distribution of the polymer can be broadened and branched long chains can be provided.

[0042] The preparation method of the ternary hydrocarbon rubber of the present invention comprises the following steps:

[0043] 1) Add a cyclohexane solution containing a quantitative structure regulator to a clean steel polymerization kettle, then heat the solution to 50-55°C, and then continuously and evenly add olefin monomers and n-butyl lithium (NBL) to the polymerization kettle within 30-40 minutes. After the monomers are added, add DVB cyclohexane solution within 1 minute and continue to react for 12-20 minutes to obtain a polymer glue. During this period, if necessary, introduce cooling water to remove the reaction heat and maintain the polymerization temperature not higher than 65°C. Finally, pressurize the glue into a hydrogenation kettle with nitrogen.

[0044] 2) Add a certain amount of NBL to the hydrogenation kettle containing the polymer glue, and then stir and activate it at 50-80° C. and 10-13 bar hydrogen pressure for 5-15 minutes, then add a certain amount of methyl phthalate cyclohexane solution to activate it for another 10-20 minutes; then add a certain amount of dicyclopentadiene titanium dichloride to hydrogenate at 13-15 bar and 70-95° C. until the unsaturation of the polymer is 1.0-2.0%, then stop hydrogenation, finally stop the hydrogenation of the glue, add a small amount of antioxidant, and condense, dehydrate and dry it to obtain block EPBR raw rubber.

[0045] The EPBR raw rubber of the present invention can be mixed, processed and vulcanized with fillers just like the existing general-purpose EPDM and conjugated diene rubbers.

[0046] The invention also provides an application of the ternary hydrocarbon rubber, which is applied to inner tube rubber material.

[0047] As a preferred solution, the inner tube rubber material includes ternary hydrocarbon rubber, butyl rubber and auxiliary materials.

[0048] As a more preferred solution, the inner tube rubber material includes the following components in parts by mass: 35-45 parts of ternary hydrocarbon rubber, 55-65 parts of butyl rubber, 0.5-1.5 parts of stearic acid, 3-8 parts of zinc oxide, 65-75 parts of carbon black, 20-30 parts of rubber oil, 1-2 parts of antioxidant, 2-3 parts of accelerator, and 1.5-1.7 parts of sulfur.

[0049] As a preferred solution, the butyl rubber is a conventional commercially available butyl rubber, such as at least one of the halogenated or non-halogenated types of IIR-268, IIR365, IIR4266, IIR-1751, etc.

[0050] As a preferred solution, the stearic acid, zinc oxide and sulfur in the inner tube rubber material are all additives known to those skilled in the art.

[0051] As a preferred solution, the rubber oils are all white oils known to those skilled in the art, and the most preferred ones are cycloalkyl or paraffin-based white oils, such as at least one of the commercially available white oils KN4010, KN4006, 46#, 32#, 400N and 320#.

[0052] As a preferred solution, the carbon black is mainly used as a reinforcing agent, and is preferably nano-scale such as N330.

[0053] As a preferred solution, the antioxidant is an amine antioxidant known to those skilled in the art, such as antioxidant 4020.

[0054] As a preferred solution, the accelerator is preferably a composite rapid vulcanization accelerator. The composite rapid vulcanization accelerator is beneficial to accelerate vulcanization, shorten vulcanization time, increase crosslinking density and improve the heat resistance of vulcanized rubber. The preferred accelerator is composed of accelerator DM and accelerator T, and the composition mass ratio is 5 to 8:1.5 to 1.7.

[0055] The preparation method of the inner tube rubber material of the present invention is an existing conventional method, which is specifically as follows: EPBR and IIR raw rubber are put into an open mixer (or internal mixer), and then the motor is started to mix, break and roll the raw rubber, and then stearic acid, zinc oxide, carbon black, white oil, antioxidant and accelerator are added in sequence for mixing, and after the powder is completely "eaten up", sulfur is added for mixing, and then the rubber is cut 3 / 4 left and right for 3 times, and then the masterbatch is thinned 6 times, and then the sheet can be taken out.

[0056] The conditions for vulcanizing the inner tube rubber material of the present invention are: the vulcanization temperature is 160° C. and the vulcanization time is 30 minutes.

[0057] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0058] The invention aims at the following problems: the ethylene propylene diene monomer (EPDM) rubber in the prior art has low side methyl content in the molecular chain, the polymer is easy to crystallize, has large deformation, and has poor air tightness compared with IIR; the double bonds in the molecular side chains vulcanize quickly, which does not match the co-vulcanization rate of the linear double bonds in the butyl rubber molecular chain, resulting in long vulcanization time and poor physical and mechanical properties; at the same time, the EPDM rubber in the prior art has the defects of long polymerization reaction time, low conversion rate of monomers, especially propylene, inability to fully convert the monomers, and requiring steps such as degassing, distillation drying, and recovery from the rubber liquid, as well as a long preparation process.

[0059] The EPBR molecular chain provided by the present invention mainly contains straight chain and side branch double bonds, which match the co-vulcanization rate of butyl rubber, have good vulcanization effect, and can form a stable and uniform vulcanization network density after co-vulcanization with the straight chain double bonds in the butyl rubber molecular chain. The vulcanized rubber has excellent comprehensive physical and mechanical properties, the density of the side alkyl in the molecular chain is higher than the side methyl of the existing EPDM molecule, the steric hindrance effect of the side alkyl hinders the thermal motion of the molecule, and its shielding effect is much greater than the shielding effect of the side methyl of the EPDM molecule, embodies excellent air tightness, and also has low crystallinity, low deformation and high resilience. The EPBR vulcanized rubber also has excellent anti-aging performance, while butyl rubber is mainly degraded and aged, and EPDM is cross-linked and aged. The aging mechanism of EPBR is the coexistence of degradation and cross-linked aging, and its hardness presents a trend of slowly rising, which makes up for the disadvantages of softening, stickiness and swelling in the later aging process of butyl rubber in the use process.

[0060] The EPBR provided by the invention has a wide molecular weight distribution, exhibits good processing performance and high filling performance, makes up for the shortcomings of butyl rubber being sticky and sticking to the roller during mixing, and improves the mixing, processing and vulcanization molding of the composite material.

[0061] The EPBR provided by the present invention is used as a material for inner tubes, retains the advantages of the original butyl rubber / EPDM composite material, has good processing performance, and the vulcanized rubber not only has excellent physical properties, but is also comparable to the existing EPDM in terms of heat resistance and anti-aging performance, but avoids various technical deficiencies in the inner tube preparation process of the existing butyl rubber / EPDM and drawbacks in the use process.

[0062] The preparation method of the EPBR and inner tube of the present invention is simple, can be produced by utilizing existing mature technology, and is easy to control and industrialize. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 This is the GPC spectrum of hydrogenated polymer EPBR-1# raw rubber.

[0064] Figure 2 H is the hydrogenated polymer EPBR-4# 1 -NMR.

[0065] Note: H 1 - In the NMR spectrum, the protons with chemical shifts of 5.573 to 5.373 are protons on -CH=CH-, and the protons with chemical shifts of 4.995 to 4.956 are protons on -CH=CH 2 . DETAILED DESCRIPTION

[0066] The following examples are intended to further illustrate the present invention in detail and are not intended to limit the scope of protection of the claims of the present invention.

[0067] In the following examples, the number average molecular weight and molecular weight distribution index of the polymers were determined by gel permeation chromatography (GPC); 1 -NMR spectrum is used to quantitatively determine the microstructure of the polymer; the mechanical properties of the vulcanized rubber are tested according to the GB / T36089-2018 method; the Mooney viscosity of the raw rubber is implemented according to the GB1232 standard; the air tightness analysis of the inner tube is tested according to the GB / T1703-2017 method.

[0068] Example 1

[0069] Under nitrogen protection, 3500 mL of cyclohexane and 0.8 mL of tetrahydrofurfuryl alcohol ethyl ether (ETE) were added to a 5L polymerization kettle, stirring was started and the material temperature was raised to 51°C. At this time, 5.0 mL of 0.65 mol / L NBL and a mixed monomer consisting of 550 mL of butadiene and 20 mL of isoprene were continuously added to the polymerization kettle respectively, and the continuous feeding time of the two was 30 min. After the materials were added, 2.0 mL of cyclohexane solution with a mass fraction of 10% divinylbenzene (DVB) was immediately added to the polymerization kettle and polymerization was continued for another 20 min, during which the polymerization temperature was maintained at no more than 65°C.

[0070] The rubber liquid was pressed into the hydrogenation kettle with nitrogen, and 8 mL of 0.65 mol / L NBL was added, the temperature was raised to 75°C, and the butyl lithium was converted into lithium hydride by stirring and activating for 10 minutes under 13 bar hydrogen pressure, followed by adding 8 mL of 0.02 mol / L cyclohexane solution of dimethyl phthalate and methyl o-toluate (cocatalyst) and activating for another 10 minutes, and then 0.32 g of dicyclopentadiene titanium dichloride was added, and the maximum temperature did not exceed 105°C under 15 bar hydrogen pressure, and the stirring was continued for 110 minutes until the unsaturation of the polymer reached 1.5%, and the hydrogenation was stopped. After the hydrogenated rubber liquid was terminated by water, a small amount of antioxidant was added, and after condensation, dehydration and drying, 348 g of block EPBR raw rubber was obtained, which was marked as EPBR-1#. The behavior analysis of the polymer is shown in Table 1.

[0071] Example 2

[0072] The relevant process conditions of Example 1 were kept unchanged, and only 540 mL of butadiene, 25 mL of isoprene, 0.9 mL of ETE, 6.5 mL of NBL, and 2.5 mL of DVB cyclohexane solution were added. The obtained hydrogenated rubber was calibrated as EPBR-2#, and the behavior analysis of the polymer is shown in Table 1.

[0073] Example 3

[0074] The relevant process conditions in Example 1 remain unchanged, except that 470 mL of butadiene, 15 mL of 1,3,5-hexatriene, 1.0 mL of tetrahydrofurfuryl alcohol hexyl ether, 6.0 mL of NBL, and 3 mL of DVB cyclohexane solution are added; the hydrogenation pressure of the hydrogenation unit is 13 bar, and the hydrogenation time is 130 min. The raw rubber obtained is calibrated as EPBR-3#, and the behavior analysis of the polymer is shown in Table 1.

[0075] Example 4

[0076] The relevant process conditions in Example 1 remain unchanged, except that 470 mL of butadiene, 30 mL of p-methylstyrene, 1.2 mL of tetrahydrofurfuryl alcohol hexyl ether, 5.5 mL of NBL, 1.8 mL of DVB cyclohexane solution, and 40 min of NBL and monomer addition time are added. The hydrogenation pressure of the hydrogenation unit is 13 bar, and the hydrogenation time is 140 min. The raw rubber obtained is calibrated as EPBR-4#, and the behavior analysis of the polymer is shown in Table 1.

[0077] Embodiment 5 (comparative example)

[0078] The relevant process conditions in Implementation 1 remain unchanged, only the monomers and NBL are added to the polymerization reactor at one time, and the hydrogenation time is 90 minutes.

[0079] The raw rubber obtained was calibrated as EPBR-5#, and the behavior analysis of the polymer is shown in Table 1.

[0080] Table 1 Analysis of characteristics of polymers in EPBR raw material source examples and commercially available EPDM

[0081]

[0082]

[0083] Note: The Mooney viscosity of EPDM4770 is tested at 125℃, and the other polymers are tested at 100℃.

[0084] Inner tube preparation embodiment

[0085] EPBR-1#, EPBR-2#, EPBR-3#, EPBR-4#, EPBR-5# in Table 1, EPDM4045 produced by Mitsui Co., Ltd. and DOW4770 raw rubber produced by DOW Chemical Co., Ltd. were mixed and vulcanized on an open mill according to the materials in the inner tube formula of the present invention. The vulcanization condition is 160°C / 30min. The formula of each embodiment is shown in Table 2, and the physical properties are shown in Table 3.

[0086] Table 2 Inner tube formula (mass fraction)

[0087]

[0088] Note: The other fillers and small materials in the formula are stearic acid 1, zinc oxide 5, carbon black 70, antioxidant 40201.5 Table 3 Physical properties of inner tube

[0089]

[0090]

[0091] Note: The curing time (Tc90) of EPDM4045 is 10.3min, and the Tc90 of EPBR-1# is 13.1min.

Claims

1. A ternary hydrocarbon rubber, characterized in that: With the following structural expression: in, R1 and R2 are independently selected from hydrogen or C1-C3 alkyl; R3 and R4 are independently selected from hydrogen, C1-C3 alkyl or vinyl; Ar is phenyl or substituted phenyl; x, n, y, m and z are the degree of polymerization, x, n, y, m and z are all greater than or equal to 0, and the sum of x, n, y and m is greater than 0, (x+y+z) / (m+n)=49-99; The unsaturation degree of the ternary hydrocarbon rubber by iodine value method is 1.0-2.0%, and the mass proportion of the side alkyl chain is not less than 65%.

2. The ternary hydrocarbon rubber according to claim 1, characterized in that: The Mooney viscosity ML of the ternary hydrocarbon rubber 100 ℃=40~55, molecular weight distribution index M w / M n Greater than 1.8, crystallinity <0.

3.

3. A method for preparing a ternary hydrocarbon rubber according to claim 1 or 2, characterized in that: After heating the polymerization solution system containing the structure regulator to the temperature required for initiating polymerization, continuously and evenly add olefin monomers and alkyl lithium to initiate and carry out polymerization reaction; after the olefin monomers and alkyl lithium are added, immediately add divinylbenzene to continue the polymerization reaction to obtain a polymer glue; first add alkyl lithium to the polymer glue for hydrogenation activation, and then add a hydrogenation catalyst to carry out catalytic hydrogenation reaction to obtain the polymer glue.

4. The method for preparing a ternary hydrocarbon rubber according to claim 3, characterized in that: The structure regulator includes at least one of difunctional ethers such as tetrahydrofurfuryl alcohol ethyl ether, ditetrahydrofurfuryl propane, tetrahydrofurfuryl alcohol butyl ether and tetrahydrofurfuryl alcohol hexyl ether.

5. A method for preparing a ternary hydrocarbon rubber according to claim 3 or 4, characterized in that: The concentration of the structure regulator in the polymerization solution system is 200-260 mg / kg solvent.

6. The method for preparing a ternary hydrocarbon rubber according to claim 3, characterized in that: The olefin monomers include conjugated diene monomers, or conjugated diene monomers and aromatic vinyl monomers; The conjugated diene monomers include and / or The aromatic vinyl monomers include wherein R5 is selected from hydrogen, C1-C3 alkyl or vinyl; Ar is selected from phenyl or substituted phenyl.

7. The method for preparing a ternary hydrocarbon rubber according to claim 3, characterized in that: The olefin monomer and alkyl lithium are continuously and uniformly added into the polymerization solution system within 30 to 40 minutes.

8. The method for preparing a ternary hydrocarbon rubber according to claim 3, characterized in that: The initiation temperature of the polymerization reaction is 50-55°C, and the maximum temperature does not exceed 65°C.

9. The method for preparing a ternary hydrocarbon rubber according to claim 3, characterized in that: The polymerization reaction is continued for 12 to 20 minutes after the divinylbenzene is added.

10. The method for preparing a ternary hydrocarbon rubber according to claim 3, characterized in that: The conditions for hydrogenation activation are: the amount of alkyl lithium added to the polymer glue is 10-15 mmol / kg, the temperature is 50-80° C., the hydrogen pressure is 10-13 bar, and the activation time is 5-15 min.

11. The method for preparing a ternary hydrocarbon rubber according to claim 3, characterized in that: The conditions of the catalytic hydrogenation reaction are: using dimethyl phthalate and / or methyl o-toluate as a co-catalyst, dicyclopentadiene titanium dichloride as a main catalyst, a hydrogen pressure of 13-15 bar, a temperature of 70-95° C., and a hydrogenation end point of a polymer unsaturation of 1.0-2.0%.

12. The method for preparing a ternary hydrocarbon rubber according to claim 11, characterized in that: The amount of the main catalyst added to the polymer colloid is 3.0-4.0 mmol / kg, and the molar ratio of the main catalyst to the co-catalyst is 7-10.

13. The use of a ternary hydrocarbon rubber according to claim 1 or 2, characterized in that: Applied to inner tube rubber.

14. The use of a ternary hydrocarbon rubber according to claim 13, characterized in that: The inner tube rubber material comprises ternary hydrocarbon rubber, butyl rubber and auxiliary materials.

15. The use of a ternary hydrocarbon rubber according to claim 14, characterized in that: The inner tube rubber material comprises the following components by weight: 35-45 parts of ternary hydrocarbon rubber, 55-65 parts of butyl rubber, 0.5-1.5 parts of stearic acid, 3-8 parts of zinc oxide, 65-75 parts of carbon black, 20-30 parts of rubber oil, 1-2 parts of antioxidant, 2-3 parts of accelerator, and 1.5-1.7 parts of sulfur.

Citation Information

Patent Citations

  • All-steel giant-scale engineering tyre side glue and all-steel giant-scale engineering tyre using the same

    CN101117409A

  • Partially hydrogenated styrene-b-butadiene-divinyl benzene / isoprene random copolymer as well as preparation and application thereof

    CN111718453A

  • Rubber composition for tire inner liner

    JP2009132835A